Cluster structure precursor and preparation method and application thereof

By adopting the cauliflower-like structure and gradient doping technology of cluster structure precursors in the field of lithium-ion batteries, the problem of insufficient performance of traditional precursors is solved, and the preparation of high-performance positive electrode materials is realized, with a larger specific surface area and higher machinery strength.

CN115893517BActive Publication Date: 2024-11-26TIANJIN B&M SCI & TECH LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211303125.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-24
Publication Date
2024-11-26
Estimated Expiration
2042-10-24

AI Technical Summary

Technical Problem

The morphology, internal structure, components, particle size, tap density and specific surface area of ​​the traditional precursor are low, resulting in poor performance of the prepared positive electrode material.

Method used

The cluster structure precursor is adopted to form spherical particles with cauliflower-like structures, including slat-shaped whiskers, by co-precipitation reaction in alkaline solution, which improves the compaction density and specific surface area of ​​the precursor, and adjusts the reaction conditions. Form a gradient doped structure.

Benefits of technology

The preparation of high-performance positive electrode materials is realized, with larger specific surface area, higher reactive activity, better lithium ion diffusion path, better rate performance and higher mechanical strength, reducing battery internal resistance and polarization losses .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115893517B_ABST
    Figure CN115893517B_ABST
Patent Text Reader

Abstract

The present application relates to a cluster structure precursor and its preparation method and application. The cluster structure precursor includes multiple clusters of spherical particles, the spherical particles include multiple lath-shaped whiskers, the lath-shaped whiskers are aggregated with each other, and multiple spherical particles are clustered into a cauliflower-like structure. Compared with the spherical precursors of the same particle size, the cauliflower-like structure precursor has a larger specific surface area and greater reaction activity, which can make the prepared positive electrode fully contact with the electrolyte to shorten the lithium ion diffusion path, and the rate performance and discharge capacity are better. The positive electrode material sintered using the cluster structure precursor can maintain a cauliflower-like morphology, the overall mechanical strength of the material is high, the gaps between particles can be reduced, the compaction density is high, and the battery internal resistance and polarization loss are small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a cluster structure precursor and a preparation method and application thereof. Background Art

[0002] The precursor is the front-end material of the positive electrode of the lithium battery, which can be processed into the positive electrode. The positive electrode can be prepared into a lithium battery by adding negative electrode materials, electrolytes, separators and other materials. At present, the preparation of conventional materials is to first prepare the precursor by co-precipitation, and then prepare the positive electrode material by high-temperature calcination. The morphology, internal structure, composition, particle size, tap density, specific surface area and other parameters of the precursor largely determine the performance of the positive electrode material product. Traditional precursors are mostly spherical precursors with relatively low compacted density and specific surface area, which is not conducive to the preparation of high-performance positive electrode materials. Summary of the invention

[0003] Based on this, it is necessary to provide a cluster structure precursor and a preparation method and application thereof, so as to achieve a precursor with relatively high compaction density and specific surface area, and thus obtain a positive electrode material with better performance.

[0004] In a first aspect, the present application provides a cluster structure precursor, comprising a plurality of clusters of spherical particles, wherein the spherical particles include a plurality of lath-like whiskers, wherein the lath-like whiskers are aggregated with each other, and the plurality of spherical particles are clustered into a cauliflower-like structure.

[0005] In some embodiments, the number of the spherical particles in the cauliflower-like structure is 2 to 30.

[0006] In one embodiment, the length of the lath-shaped whiskers is 200-600 nm.

[0007] In one embodiment, the thickness of the lath-shaped whiskers is 20-150 nm.

[0008] In some embodiments, the chemical formula of the cluster structure precursor is: (Ni x Co y Mn z ) 1-a M a (OH) b , wherein 0.50≤x≤1.0, 0≤y≤0.30, 0≤z≤0.30, x+y+z=1, 0.00001≤a≤0.30, b is determined according to the valence state of M and a; M includes one or more of Mg, Al, Zr, Ti, Y, Sr, Nb, W and Mo.

[0009] In some embodiments, the concentration of the M element gradually increases along the direction from the inside to the outside of the cluster structure precursor.

[0010] In one embodiment, the particle size D50 of the cluster structure precursor is 2 to 6 μm.

[0011] In one embodiment, the particle size distribution diameter distance K90 of the cluster structure precursor is ≥1.

[0012] In one embodiment, the tap density of the cluster structure precursor is ≥1.4 g / cm 3 .

[0013] In one embodiment, the specific surface area of ​​the cluster structure precursor is ≥18m 2 / g.

[0014] In a second aspect, the present application also provides a method for preparing a cluster structure precursor according to any of the above-mentioned methods, comprising: forming a plurality of clusters of spherical particles, so that the plurality of clusters of the spherical particles form a cauliflower-like structure, wherein the spherical particles include a plurality of lath-like whiskers, and the lath-like whiskers are aggregated with each other.

[0015] In some embodiments, the forming of multiple clusters of spherical particles so that the multiple clusters of spherical particles form a cauliflower-like structure includes: under a protective gas atmosphere, co-precipitating a mixed salt, a thickener, and an ammonia complexing agent in an alkaline solution; the mixed salt includes one or more of Ni, Co, and Mn and at least contains Ni, and the thickener includes one or more of Mg, Al, Zr, Ti, Y, Sr, Nb, W, and Mo.

[0016] In some embodiments, the co-precipitation reaction of the mixed salt, thickener and ammonia complexing agent in an alkaline solution comprises: adding the mixed salt solution, thickener solution, ammonia complexing agent solution and alkaline solution to a reaction container at flow rates Q1, Q2, Q3 and Q4, respectively, and performing a first mixing reaction to obtain the quasi-spherical particles; when the particle size of the quasi-spherical particles reaches a preset particle size, adjusting the flow rates of the mixed salt solution, the thickener solution, the ammonia complexing agent solution and the alkaline solution, respectively, and performing a second mixing reaction; wherein adjusting the flow rates of the mixed salt solution, the thickener solution, the ammonia complexing agent solution and the alkaline solution, respectively, comprises: linearly increasing Q1 to Q2 with time t1; 11 , the Q2 increases linearly with time t2 to Q 21 , the Q3 increases linearly with time t3 to Q 31 , the Q4 is linearly reduced to Q with time t4 41 .

[0017] In one embodiment, Q 21 :Q2>Q 11 :Q1.

[0018] In one embodiment, the coprecipitation reaction further comprises stirring, and when the particle size of the spherical particles reaches a preset particle size, the stirring speed is adjusted; wherein the stirring speed in the first mixing reaction is r1, and adjusting the stirring speed comprises: linearly reducing r1 to r2 over time t5. In one embodiment, the reaction temperature of the first mixing reaction is 50-70°C.

[0019] In one embodiment, the pH value of the first mixed reaction is 11.5-12.5.

[0020] In one embodiment, the ammonia concentration of the first mixing reaction is 1-6 g / L.

[0021] In one embodiment, the reaction temperature of the second mixing reaction is 50-70°C.

[0022] In one embodiment, the pH value of the second mixed reaction is 10.5-11.2.

[0023] In one embodiment, the ammonia concentration of the second mixing reaction is 6-15 g / L.

[0024] In a third aspect, the present application further provides a positive electrode material, wherein raw materials for preparing the positive electrode material include a lithium source and a cluster structure precursor according to any one of the above.

[0025] In a fourth aspect, the present application also provides a positive electrode plate, comprising a current collector and an active layer located on at least one surface of the current collector, wherein the active layer comprises the above-mentioned positive electrode material.

[0026] In a fifth aspect, the present application also provides a lithium-ion battery, comprising the above-mentioned positive electrode plate.

[0027] In the above-mentioned cluster structure precursor, multiple quasi-spherical particle clusters form a cauliflower-like structure, and the quasi-spherical particles include multiple lath-like whiskers, and the lath-like whiskers are aggregated with each other. The cluster structure precursor has the characteristics of good uniformity of lath-like whiskers, multiple spherical particle clusters forming a non-spherical cauliflower-like structure, high compaction density, and high volume energy density. Compared with spherical particles of the same particle size, cauliflower-like precursors have a larger specific surface area and greater reaction activity, which can make the prepared positive electrode fully contact with the electrolyte to shorten the lithium ion diffusion path, and have better rate performance and discharge capacity. The positive electrode material sintered using the cluster structure precursor can maintain a cauliflower-like morphology, the overall mechanical strength of the material is high, the gaps between particles can be reduced, the compaction density is high, and the battery internal resistance and polarization loss are small.

[0028] The above-mentioned method for preparing the cluster structure precursor can prepare a precursor with relatively high compaction density and specific surface area, thereby obtaining a positive electrode material with better performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of a process for preparing a cluster structure precursor provided for an embodiment of the present application;

[0030] Figure 2 This is a scanning electron microscope image of the cluster structure precursor provided in Example 1 of the present application;

[0031] Figure 3 This is a scanning electron microscope image of the cluster structure precursor provided in Example 2 of the present application;

[0032] Figure 4 This is a scanning electron microscope image of the cluster structure precursor provided in Example 3 of the present application. DETAILED DESCRIPTION

[0033] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0035] An embodiment of the present application provides a cluster structure precursor, including a plurality of clusters of spherical particles, including a plurality of lath-shaped whiskers, the lath-shaped whiskers are aggregated with each other, and the plurality of spherical particles are clustered into a cauliflower-like structure.

[0036] In the cluster structure precursor, multiple quasi-spherical particle clusters form a cauliflower-like structure, and the quasi-spherical particles include multiple lath-like whiskers, and the lath-like whiskers are aggregated with each other. The cluster structure precursor has the characteristics of good uniformity of lath-like whiskers, multiple spherical particle clusters forming a non-spherical cauliflower-like structure, high compaction density, and high volume energy density. Compared with spherical particles of the same particle size, the cauliflower-like precursor has a larger specific surface area and greater reaction activity, which can make the prepared positive electrode fully contact with the electrolyte to shorten the lithium ion diffusion path, and has better rate performance and discharge capacity. The positive electrode material sintered using the cluster structure precursor can maintain a cauliflower-like morphology, the overall mechanical strength of the material is high, the gaps between particles can be reduced, the compaction density is high, and the battery internal resistance and polarization loss are small.

[0037] In some embodiments, the number of spherical particles in the cauliflower-like structure is 2 to 30. Within the number range of spherical particles, the cluster structure precursor has a larger specific surface area, a higher compaction density, and a higher reaction activity. Optionally, the number of spherical particles in the cauliflower-like structure is 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 22, 25, 28 or 30.

[0038] In some embodiments, the length of the lath-shaped whiskers is 200-600 nm. Within the length range of the lath-shaped whiskers, the uniformity of the lath-shaped whiskers is good, and the clustering effect of the spherical particles is good. Optionally, the length of the lath-shaped whiskers is 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm or 600 nm.

[0039] In some embodiments, the thickness of the lath whisker is 20 to 150 nm. Within the thickness range of the lath whisker, the lath whisker has good uniformity and the clustering effect of the spherical particles is good. Optionally, the thickness of the whisker is 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm or 150 nm.

[0040] In some embodiments, the chemical formula of the cluster structure precursor is: (Ni x Co y Mn z ) 1-a M a (OH) b, wherein 0.50≤x≤1.0, 0≤y≤0.30, 0≤z≤0.30, x+y+z=1, 0.00001≤a≤0.30, b is determined according to the valence state of M and a; M includes one or more of Mg, Al, Zr, Ti, Y, Sr, Nb, W and Mo. Optionally, x is 0.5, 0.6, 0.7, 0.8, 0.9 or 1.0. Optionally, y is 0, 0.1, 0.2 or 0.3. Optionally, z is 0, 0.1, 0.2 or 0.3. Optionally, a is 0.00001, 0.0001, 0.001, 0.01, 0.1, 0.2 or 0.3.

[0041] In some embodiments, the concentration of the M element gradually increases from the inside to the outside of the cluster structure precursor. After the cluster structure precursor is sintered with the lithium source, a gradient doping of the M element can be formed, and a positive electrode material with an outer layer of M oxide and Li-MO co-modified coating can be obtained.

[0042] In some embodiments, the Ni element, the Co element, and the Mn element are uniformly distributed in the particles of the cluster structure precursor.

[0043] In some embodiments, the particle size D50 of the cluster structure precursor is 2 to 6 μm. Within the particle size D50 range of the cluster structure precursor, when the precursor is sintered with a lithium source, the obtained positive electrode material has a high mechanical strength and a high compaction density. Optionally, the particle size D50 of the cluster structure precursor is 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm or 6 μm.

[0044] In one embodiment, the particle size distribution distance K90 of the cluster structure precursor is ≥ 1. Within the particle size distribution distance K90 of the cluster structure precursor, when the precursor is sintered with a lithium source, the obtained positive electrode material has a higher mechanical strength and a higher compaction density.

[0045] In one embodiment, the tap density of the cluster structure precursor is ≥1.4 g / cm 3 Within the tap density range of the cluster structure precursor, when the precursor is sintered with a lithium source, the obtained positive electrode material has a high mechanical strength and a high compaction density.

[0046] In one embodiment, the specific surface area of ​​the cluster structure precursor is ≥18m 2 / g. The specific surface area of ​​the cluster structure precursor is ≥18m 2 / g range, when the precursor and the lithium source are sintered, the obtained positive electrode material has higher mechanical strength and higher compaction density.

[0047] Reference Figure 1Another embodiment of the present application provides a method for preparing a cluster structure precursor according to any of the above, comprising:

[0048] S101: forming a plurality of clusters of spherical particles, so that the plurality of spherical particle clusters form a cauliflower-like structure, wherein the spherical particles include a plurality of lath-like whiskers, and the lath-like whiskers are aggregated with each other.

[0049] In some embodiments, forming multiple clusters of spherical particles, and making the multiple spherical particle clusters into a cauliflower-like structure includes: in a protective gas atmosphere, co-precipitating a mixed salt, a thickener, and an ammonia complexing agent in an alkaline solution; the mixed salt includes one or more of Ni, Co, and Mn and at least contains Ni, and the thickener includes one or more of Mg, Al, Zr, Ti, Y, Sr, Nb, W, and Mo. The addition of the thickener can improve the thickening effect and optimize the cluster morphology of the cauliflower-like structure.

[0050] In some embodiments, the mixed salt, thickener and ammonia complexing agent are subjected to a coprecipitation reaction in an alkaline solution, comprising: adding the mixed salt solution, the thickener solution, the ammonia complexing agent solution and the alkaline solution to a reaction container at flow rates Q1, Q2, Q3 and Q4, respectively, and performing a first mixing reaction to obtain quasi-spherical particles; when the particle size of the quasi-spherical particles reaches a preset particle size, adjusting the flow rates of the nickel-cobalt-manganese mixed salt solution, the thickener solution, the ammonia complexing agent solution and the alkaline solution, respectively, and performing a second mixing reaction; wherein adjusting the flow rates of the mixed salt solution, the thickener solution, the ammonia complexing agent solution and the alkaline solution, respectively, comprises: linearly increasing Q1 to Q2 with time t1; 11 , increase Q2 linearly with time t2 to Q 21 , increase Q3 linearly with time t3 to Q 31 , linearly reduce Q4 to Q with time t4 41 By adopting a higher rotation speed, a lower flow rate of the mixed salt solution and the thickener solution, a higher pH, and a lower ammonia value in the initial stage, spherical particles with better sphericity are formed, and then by reducing the rotation speed, increasing the flow rate of the mixed salt solution and the thickener solution, reducing the pH, and increasing the ammonia value, the spherical particles with better sphericity are adhered to each other and grow, and a cauliflower-like cluster structure formed by multiple spherical particles adhering to each other is obtained.

[0051] In one embodiment, the shielding gas includes at least one of nitrogen, argon and helium.

[0052] In one embodiment, the alkali solution includes at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0053] In one embodiment, the ammonia complexing agent includes one or more of aqueous ammonia, urea and ammonium bicarbonate.

[0054] In one embodiment, t1 is 1 to 30 hours. Optionally, t1 is 1 hour, 3 hours, 5 hours, 10 hours, 15 hours, 20 hours, 25 hours or 30 hours.

[0055] In one embodiment, t2 is 1 to 30 hours. Optionally, t2 is 1 hour, 3 hours, 5 hours, 10 hours, 15 hours, 20 hours, 25 hours or 30 hours.

[0056] In one embodiment, t3 is 1 to 30 hours. Optionally, t3 is 1 hour, 3 hours, 5 hours, 10 hours, 15 hours, 20 hours, 25 hours or 30 hours.

[0057] In one embodiment, t4 is 1 to 30 hours. Optionally, t4 is 1 hour, 3 hours, 5 hours, 10 hours, 15 hours, 20 hours, 25 hours or 30 hours.

[0058] In one embodiment, Q 21 :Q2>Q 11 :Q1. The concentration of M element gradually increases from the inside to the outside of the cluster structure precursor.

[0059] In one embodiment, Q 21 :Q2 is 1.01 to 50. Optionally, Q 21 :Q2 is 1.01, 1.05, 1.1, 1.3, 1.5, 2, 3, 5, 10, 15, 20, 25, 30, 40 or 50.

[0060] In one embodiment, Q 11 :Q1 is 1.01 to 30. Optionally, Q 11 :Q1 is 1.01, 1.05, 1.1, 1.3, 1.5, 2, 3, 5, 10, 15, 20, 25 or 30.

[0061] In one embodiment, the coprecipitation reaction further includes stirring, and when the particle size of the spherical particles reaches a preset particle size, the stirring speed is adjusted; wherein the stirring speed in the first mixing reaction is r1, and adjusting the stirring speed includes: linearly reducing r1 to r2 over time t5.

[0062] In one embodiment, 0.01r1≤r2≤0.8r1. Within the range of r2, the clustering effect of spherical particles bonding to each other into a cauliflower-like structure is better. Optionally, r2=0.01r1, r2=0.03r1, r2=0.05r1, r2=0.1r1, r2=0.2r1, r2=0.3r1, r2=0.4r1, r2=0.5r1, r2=0.6r1, r2=0.7r1, r2=0.8r1.

[0063] In one embodiment, t5 is 0.5 to 6 hours. Optionally, t5 is 0.5 hours, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.

[0064] In one embodiment, t5 is less than the smallest of t1, t2, t3 and t4.

[0065] In one embodiment, the reaction temperature of the first mixing reaction is 50-70° C. Within the reaction temperature range of the first mixing reaction, the preparation effect of spherical particles is better. Optionally, the reaction temperature of the first mixing reaction is 50° C., 52° C., 54° C., 56° C., 58° C., 60° C., 62° C., 64° C., 66° C., 68° C. or 70° C.

[0066] In one embodiment, the pH value of the first mixing reaction is 11.5 to 12.5. Within the pH value range of the first mixing reaction, the preparation effect of spherical particles is better. Optionally, the pH value of the first mixing reaction is 11.5, 11.6, 11.7, 11.8, 11.9, 12, 12.1, 12.2, 12.3, 12.4 or 12.5.

[0067] In one embodiment, the ammonia concentration of the first mixing reaction is 1 to 6 g / L. Within the range of the ammonia concentration of the first mixing reaction, the preparation effect of spherical particles is better. Optionally, the ammonia concentration of the first mixing reaction is 1 g / L, 2 g / L, 3 g / L, 4 g / L, 5 g / L or 6 g / L.

[0068] In one embodiment, the reaction temperature of the second mixing reaction is 50-70° C. Within the reaction temperature range of the second mixing reaction, the clustering of multiple spherical particles into a cauliflower-like structure has a better effect. Optionally, the reaction temperature of the second mixing reaction is 50° C., 55° C., 60° C., 65° C. or 70° C.

[0069] In one embodiment, the pH value of the second mixed reaction is 10.5 to 11.2. Within the pH value range of the second mixed reaction, the clustering of multiple spherical particles into a cauliflower-like structure has a better effect. Optionally, the pH value of the second mixed reaction is 10.5, 10.6, 10.7, 10.8, 10.9, 11, 11.1 or 11.2.

[0070] In one embodiment, the ammonia concentration of the second mixing reaction is 6 to 15 g / L. Within the ammonia concentration range of the second mixing reaction, a plurality of spherical particles clustered into a cauliflower-like structure has a better effect. Optionally, the ammonia concentration of the second mixing reaction is 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L or 15 g / L.

[0071] In one embodiment, the method for preparing the cluster structure precursor comprises:

[0072] S201: preparing a mixed salt solution of nickel salt, cobalt salt and manganese salt, and preparing a thickener solution, an ammonia complexing agent solution and an alkali solution.

[0073] S202: Under a protective gas atmosphere, a mixed salt solution, a thickener solution, an alkali solution and an ammonia complexing agent are added into a reaction container at flow rates Q1, Q2, Q3 and Q4, respectively, to carry out a first mixing reaction to obtain spherical particles.

[0074] S203: When the size of the spherical particles reaches the preset size, Q1 is linearly increased to Q 11 , increase Q2 linearly with time t2 to Q 21 , increase Q3 linearly with time t3 to Q 31 , linearly reduce Q4 to Q with time t4 41 And carry out the second mixing reaction.

[0075] In one embodiment, the concentration of the mixed salt solution is 1.2-2.7 mol / L. Optionally, the concentration of the mixed salt solution is 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, 2.0 mol / L, 2.3 mol / L, 2.5 mol / L or 2.7 mol / L.

[0076] In one embodiment, the concentration of the thickener solution is 1.2-2.7 mol / L. Optionally, the concentration of the thickener solution is 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, 2.0 mol / L, 2.3 mol / L, 2.5 mol / L or 2.7 mol / L.

[0077] In one embodiment, the concentration of the alkali solution is 1 to 13 mol / L. Optionally, the concentration of the alkali solution is 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L or 13 mol / L.

[0078] In one embodiment, the concentration of the ammonia complexing agent solution is 1 to 12 mol / L. Optionally, the concentration of the ammonia complexing agent solution is 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L or 13 mol / L.

[0079] In one embodiment, after the second mixing reaction, the material is further aged, solid-liquid separated, washed, dried, screened and demagnetized. Aging means stopping the addition of samples and continuing stirring.

[0080] In one embodiment, the aging time is 1 to 2 hours. Optionally, the aging time is 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours.

[0081] Another embodiment of the present application provides a positive electrode material, and raw materials for preparing the positive electrode material include a lithium source and any of the above-mentioned cluster structure precursors.

[0082] In one embodiment, the positive electrode material is sintered by a cluster structure precursor and a lithium source, and the sintering temperature is 700-950° C. Optionally, the sintering temperature is 700° C., 750° C., 800° C., 850° C., 900° C. or 950° C. Optionally, the lithium source includes one or more of LiOH, Li2CO3, LiNO3, lithium oxalate, and lithium acetate.

[0083] Another embodiment of the present application provides a positive electrode plate, including a current collector and an active layer located on at least one surface of the current collector, wherein the active layer includes the above-mentioned positive electrode material.

[0084] Another embodiment of the present application provides a lithium-ion battery, comprising the above-mentioned positive electrode plate.

[0085] The following are specific embodiments.

[0086] Example 1

[0087] In this embodiment, the chemical formula of the cluster structure precursor is (Ni 0.9 Co 0.1 ) 0.99 Al 0.01 (OH) 2.01 , the corresponding cathode material is Li 1.02 (Ni 0.9 Co 0.1 ) 0.99 Al 0.01 O2.

[0088] Preparation of cluster structure precursors:

[0089] (1) nickel chloride and cobalt chloride are taken at a molar ratio of 9:1 to prepare a mixed salt solution with a concentration of 1.2 to 2.7 mol / L, sodium aluminate is taken to prepare a thickener solution with a concentration of 1.2 to 2.7 mol / L, sodium hydroxide is taken to prepare an alkali solution with a concentration of 1.0 to 13.0 mol / L, and ammonia water with a concentration of 1.0 to 12.0 mol / L is prepared.

[0090] (2) Nitrogen is introduced into the reaction container until it is full, and a set amount of pure water is added, and then alkali solution and ammonia water are added to form a reaction start-up base liquid with a pH of 12.5 and an ammonia concentration of 3.0 g / L.

[0091] (3) Nitrogen was continuously introduced, and the mixed salt solution, thickener solution, alkali solution and ammonia water were added into the reaction container at a stirring speed of 200 rpm for stirring and reacting, and the reaction temperature was controlled to be 60.0° C., the pH value was 12.5, and the ammonia concentration was 3.0 g / L to form spherical particles.

[0092] (4) When the particle size of the spherical particles in the container reaches the set value, the reaction temperature is controlled to 60.0°C, the flow rate of the alkali solution is linearly reduced to a pH of 10.5 over a period of 10 hours, the flow rate of the ammonia water is linearly increased to an ammonia concentration of 9.0 g / L over a period of 10 hours, the flow rate of the mixed salt solution is linearly adjusted to 5 times that in step (3) over a period of 10 hours, the flow rate of the thickener solution is linearly adjusted to 10 times that in step (3) over a period of 10 hours, the rotation speed is linearly reduced to 80 rpm over a period of 2 hours, and when it is detected that the particle size of the material in the reaction container reaches 6 μm, the feeding is stopped, and stirring and aging is continued for 1 to 2 hours.

[0093] (5) The aged material is subjected to solid-liquid separation, washing, drying, screening and demagnetization to obtain a cluster structure precursor.

[0094] Preparation of positive electrode materials:

[0095] The cluster structure precursor prepared above and the lithium source (calculated as lithium) were mixed uniformly in a high-speed mixer at a molar ratio of 1.02:1, and sintered at 720° C. for 9 hours in an oxygen atmosphere to obtain a positive electrode material.

[0096] The particle size D50 of the prepared cluster structure precursor was determined by laser particle size analysis diffraction method to be 6 μm. Figure 1 The cluster structure precursor prepared in Example 1 is a cauliflower-like structure composed of multiple spherical particle clusters, and has a large specific surface area.

[0097] Example 2

[0098] In this embodiment, the chemical formula of the cluster structure precursor is (Ni 0.7 Co 0.1 Mn 0.2 ) 0.995 Zr 0.005 (OH) 2.01 , the corresponding cathode material is Li 1.04 (Ni 0.7 Co 0.1 Mn 0.2 ) 0.995 Zr 0.005 O2.

[0099] Preparation of cluster structure precursors:

[0100] (1) Nickel, cobalt and manganese sulfates are taken respectively in a molar ratio of 7:1:2 to prepare a mixed salt solution with a concentration of 1.2 to 2.7 mol / L, zirconium sulfate is taken to prepare a thickener solution with a concentration of 1.2 to 2.7 mol / L, potassium hydroxide is taken to prepare an alkali solution with a concentration of 1.0 to 13.0 mol / L, and ammonia water with a concentration of 1.0 to 12.0 mol / L is prepared.

[0101] (2) Nitrogen is introduced into the reaction container until it is full, and a set amount of pure water is added, and then alkali solution and ammonia water are added to form a reaction start-up bottom liquid with a pH of 12.2 and an ammonia concentration of 4.0 g / L.

[0102] (3) Nitrogen was continuously introduced, and the mixed salt solution, thickener solution, alkali solution and ammonia water were added into the reaction container at a stirring speed of 180 rpm to react, and the reaction temperature was controlled to be 65.0° C., the pH value was 12.2, and the ammonia concentration was 4.0 g / L to form spherical particles.

[0103] (4) When the particle size of the spherical particles in the container reaches the set value, the reaction temperature is controlled to 65.0°C, the flow rate of the alkali solution is linearly reduced to a pH of 11.1 over a period of 20 hours, the flow rate of the ammonia water is linearly increased to an ammonia concentration of 12 g / L over a period of 20 hours, the flow rate of the mixed salt solution is linearly adjusted to 10 times that in step (3) over a period of 20 hours, the flow rate of the thickener solution is linearly adjusted to 15 times that in step (3) over a period of 20 hours, the rotation speed is linearly reduced to 54 rpm over a period of 5 hours, and when the particle size of the material in the reaction container is detected to reach 3 μm, the feeding is stopped, and stirring and aging is continued for 1 to 2 hours.

[0104] (5) The aged material is subjected to solid-liquid separation, washing, drying, screening and demagnetization to obtain a cluster structure precursor.

[0105] Preparation of positive electrode materials:

[0106] The cluster structure precursor prepared above and the lithium source (calculated as lithium) were mixed uniformly in a high-speed mixer at a molar ratio of 1.04:1, and sintered at 800° C. for 12 h in an oxygen atmosphere to obtain a positive electrode material.

[0107] The particle size D50 of the prepared cluster structure precursor was determined by laser particle size analysis diffraction method to be 3 μm. Figure 2 The cluster structure precursor prepared in Example 2 is a cauliflower-like structure composed of multiple spherical particle clusters, and has a large specific surface area.

[0108] Example 3

[0109] In this embodiment, the chemical formula of the cluster structure precursor is (Ni 0.6 Co 0.1 Mn 0.3 ) 0.99 Al 0.002 Zr 0.008 (OH) 2.02 , the corresponding cathode material is Li 1.08 (Ni 0.6 Co 0.1 Mn 0.3 ) 0.99 Al 0.002 Zr 0.008 O2.

[0110] Preparation of cluster structure precursors:

[0111] (1) Nitrates of nickel, cobalt and manganese are taken at a molar ratio of 6:1:3 to prepare a mixed salt solution with a concentration of 1.2 to 2.7 mol / L, zirconium nitrate and aluminum nitrate are taken at a molar ratio of 8:2 to prepare a thickener solution with a concentration of 1.2 to 2.7 mol / L, potassium hydroxide is taken to prepare an alkali solution with a concentration of 1.0 to 13.0 mol / L, and ammonia water with a concentration of 1.0 to 12.0 mol / L is prepared.

[0112] (2) Nitrogen is introduced into the reaction container until it is full, and a set amount of pure water is added, and then alkali solution and ammonia water are added to form a reaction start-up bottom liquid with a pH of 12.2 and an ammonia concentration of 4.0 g / L.

[0113] (3) Nitrogen was continuously introduced, and the mixed salt solution, thickener solution, alkali solution and ammonia water were added into the reaction container at a stirring speed of 180 rpm to react, and the reaction temperature was controlled to be 65.0° C., the pH value was 12.2, and the ammonia concentration was 4.0 g / L to form spherical particles.

[0114] (4) When the particle size of the spherical particles in the container reaches the set value, the reaction temperature is controlled to 65.0°C, the flow rate of the alkali solution is linearly reduced to a pH of 11.1 over a period of 20 hours, the flow rate of the ammonia water is linearly increased to an ammonia concentration of 12 g / L over a period of 20 hours, the flow rate of the mixed salt solution is linearly adjusted to 10 times that in step (3) over a period of 20 hours, the flow rate of the thickener solution is linearly adjusted to 15 times that in step (3) over a period of 20 hours, the rotation speed is linearly reduced to 54 rpm over a period of 5 hours, and when the particle size of the material in the reaction container is detected to reach 3 μm, the feeding is stopped, and stirring and aging is continued for 1 to 2 hours.

[0115] (5) The aged material is subjected to solid-liquid separation, washing, drying, screening and demagnetization to obtain a cluster structure precursor.

[0116] Preparation of positive electrode materials:

[0117] The cluster structure precursor prepared above and the lithium source (calculated as lithium) were mixed uniformly in a high-speed mixer at a molar ratio of 1.08:1, and sintered at 840° C. for 9 hours in an oxygen atmosphere to obtain a positive electrode material.

[0118] The particle size D50 of the prepared cluster structure precursor was determined by laser particle size analysis diffraction method to be 3 μm. Figure 3 The cluster structure precursor prepared in Example 3 is a cauliflower-like structure composed of multiple spherical particle clusters, and has a large specific surface area.

[0119] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0120] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the description and drawings may be used to interpret the contents of the claims.

Claims

1. A cluster structure precursor, characterized in that: A plurality of clusters of spherical particles, wherein the spherical particles include a plurality of lath-shaped whiskers, the lath-shaped whiskers are aggregated with each other, and the plurality of spherical particles are clustered into a cauliflower-like structure; the number of the spherical particles in the cauliflower-like structure is 3 to 30; The length of the lath-shaped whisker is 200-600 nm; the thickness of the lath-shaped whisker is 20-150 nm; The particle size D50 of the cluster structure precursor is 2-6 μm; the particle size distribution distance K90 of the cluster structure precursor is ≥1; the tap density of the cluster structure precursor is ≥1.4 g / cm 3 ; The specific surface area of ​​the cluster structure precursor is ≥18m 2 / g.

2. The cluster structure precursor according to claim 1, characterized in that: The chemical formula of the cluster structure precursor is: (Ni x Co y Mn z ) 1-a M a (OH) b , wherein 0.50≤x≤1.0, 0≤y≤0.30, 0≤z≤0.30, x+y+z=1, 0.00001≤a≤0.30, b is determined according to the valence state of M and a; M includes one or more of Mg, Al, Zr, Ti, Y, Sr, Nb, W and Mo.

3. The cluster structure precursor according to claim 2, characterized in that: The concentration of the M element gradually increases along the direction from the inside to the outside of the cluster structure precursor.

4. A method for preparing a cluster structure precursor according to any one of claims 1 to 3, characterized in that: include: Forming a plurality of clusters of spherical particles, so that the plurality of spherical particle clusters form a cauliflower-like structure, wherein the number of the spherical particles in the cauliflower-like structure is 3 to 30, wherein the spherical particles include a plurality of lath-like whiskers, and the lath-like whiskers are aggregated with each other; The forming of a plurality of clusters of spherical particles, wherein the plurality of clusters of spherical particles are clustered into a cauliflower-like structure, comprises: Under a protective gas atmosphere, the mixed salt, the viscosity enhancer and the ammonia complexing agent are subjected to a co-precipitation reaction in an alkaline solution; The mixed salt includes one or more of Ni, Co, and Mn and contains at least Ni, and the viscosity enhancer includes one or more of Mg, Al, Zr, Ti, Y, Sr, Nb, W, and Mo.

5. The method for preparing a cluster structure precursor according to claim 4, characterized in that: The method of coprecipitating the mixed salt, the tackifier and the ammonia complexing agent in an alkaline solution comprises: Adding a mixed salt solution, a thickener solution, an ammonia complexing agent solution and an alkali solution into a reaction container at flow rates Q1, Q2, Q3 and Q4 respectively, and performing a first mixing reaction to obtain the spherical particles; When the particle size of the spherical particles reaches a preset particle size, the flow rates of the mixed salt solution, the viscosity enhancer solution, the ammonia complexing agent solution and the alkali solution are adjusted respectively and a second mixing reaction is performed; Wherein, adjusting the flow rates of the mixed salt solution, the viscosity enhancer solution, the ammonia complexing agent solution and the alkali solution respectively comprises: increasing Q1 linearly with time t1 to Q 11 , the Q2 increases linearly with time t2 to Q 21 , the Q3 increases linearly with time t3 to Q 31 , the Q4 is linearly reduced to Q with time t4 41 .

6. The method for preparing a cluster structure precursor according to claim 5, characterized in that: Q 21 :Q2>Q 11 :Q1。 7. The method for preparing a cluster structure precursor according to claim 5, characterized in that: The coprecipitation reaction also includes stirring; when the particle size of the spherical particles reaches a preset particle size, adjusting the stirring speed; wherein the stirring speed in the first mixing reaction is r1, and adjusting the stirring speed includes: linearly reducing r1 to r2 over time t5.

8. The method for preparing a cluster structure precursor according to any one of claims 5 to 7, characterized in that: The first mixing reaction satisfies at least one of the following characteristics: (1) The reaction temperature of the first mixing reaction is 50-70°C; (2) The pH value of the first mixed reaction is 11.5-12.5; (3) The ammonia concentration of the first mixing reaction is 1-6 g / L.

9. The method for preparing a cluster structure precursor according to any one of claims 5 to 7, characterized in that: The second mixing reaction satisfies at least one of the following characteristics: (1) The reaction temperature of the second mixed reaction is 50-70°C; (2) The pH value of the second mixed reaction is 10.5-11.2; (3) The ammonia concentration of the second mixing reaction is 6-15 g / L.

10. A positive electrode material, characterized in that: The raw materials for preparing the positive electrode material include a lithium source and a cluster structure precursor according to any one of claims 1 to 3.

11. A positive electrode sheet, characterized in that: The invention comprises a current collector and an active layer located on at least one surface of the current collector, wherein the active layer comprises the positive electrode material according to claim 10.

12. A lithium ion battery, characterized in that: Comprising the positive electrode sheet according to claim 11.

Citation Information

Patent Citations

  • High-nickel positive electrode material, nickel-cobalt precursor material, preparation method of high-nickel positive electrode material, preparation method of nickel-cobalt precursor material and lithium ion battery

    CN111244459A

  • Preparation method of lithium ion battery positive electrode material precursor

    CN113415830A

  • Preparation method of multigene co-agglomerated precursor for lithium battery and precursor

    CN114988495A

  • High-nickel ternary precursor and preparation method thereof

    CN115215384A