A low temperature resistant modified binary fluororubber compound and its preparation method and use

Through the preparation of modified binary fluoro-rubber mixing rubber, the combination of type 26 fluoro-rubber and other additives is used to solve the problem of insufficient cold resistance of type 26 fluoro-rubber, and the improvement of hardness, mechanical properties and low temperature resistance is achieved. Its application areas and reduces production costs.

CN115895146BActive Publication Date: 2024-11-01四川道弘新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211634648.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-11-01
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

The cold resistance of type 26 fluoroelastomer is poor, which limits its application breadth in low temperature environments, especially in the field of sealed products.

Method used

By preparing a modified binary fluoro-rubber mixing rubber, using type 26 fluoro-rubber as the basis, adding vulcanizing agent, acid absorbing agent, filler, processing auxiliary agent and white carbon black raw materials to perform specific kneading and thinning The treatment significantly increases the low-temperature brittle temperature of the material.

Benefits of technology

While maintaining the hardness and mechanical properties of Type 26 fluoroelastomer, it significantly reduces the low-temperature brittle temperature, making it reach below -35℃, improves low-temperature resistance, expands the application range, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004007060930000061
    Figure BDA0004007060930000061
Patent Text Reader

Abstract

The present invention provides a low-temperature resistant modified binary fluororubber compound and its preparation method and use, belonging to the field of polymer materials. The modified binary fluororubber compound of the present invention comprises the following raw materials in weight ratio: 100 parts of fluororubber, 1-5 parts of vulcanizing agent, 5-10 parts of acid absorber, 10-30 parts of filler, 1-5 parts of processing aid, and 5-10 parts of white carbon black. The compound of the present invention significantly reduces its low-temperature brittle temperature while maintaining the good hardness and mechanical properties of 26-type fluororubber, so that its low-temperature brittle temperature can reach below -35°C, and the low-temperature resistance effect is significantly improved. The modified fluororubber compound of the present invention has good hardness, mechanical properties and low-temperature resistance at the same time, and has excellent comprehensive performance, which can greatly expand the application of 26-type fluororubber. At the same time, the present invention can greatly reduce production costs and improve production efficiency in practical applications, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a low-temperature resistant modified binary fluororubber compound and a preparation method and application thereof. Background Art

[0002] Fluororubber (fluoro rubber) is a synthetic polymer elastomer containing fluorine atoms on the carbon atoms of the main chain or side chain, and belongs to special rubber. Fluororubber was first developed by DuPont in the United States. It developed rapidly in the 1950s and 1960s due to the arms race between the United States and the Soviet Union during the Cold War. Later, it developed rapidly with the increase in demand from the automobile industry. It has now become one of the most important products in the fluorine chemical industry. Fluororubber has excellent properties such as odorlessness, non-toxicity, non-flammability, heat resistance, oxidation resistance, oil resistance, and chemical resistance. Therefore, it occupies an important position in modern industry. Fluororubber products are mainly seals, gaskets, gaskets, diaphragms, hoses, oil seals, linings and anti-corrosion products, as well as electrical insulation products. They are currently widely used in various fields, such as the automotive industry, chemical and petroleum industries, energy industries, commercial and military aviation industries, semiconductor industries, and other fields.

[0003] According to different molecular structures, fluororubber can be divided into various types of fluororubbers such as type 23 (vinylidene fluoride-chlorotrifluoroethylene), type 26 (vinylidene fluoride-hexafluoropropylene) and type 246 (vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene). Among them, type 26 fluororubber and type 246 fluororubber are the most widely used. Type 26 fluororubber is a copolymer of vinylidene fluoride and hexafluoropropylene, with excellent heat resistance (long-term use temperature 250℃, short-term 300℃), resistance to compression permanent deformation, oil resistance, good mechanical strength and medium resistance. It is mainly used in high temperature resistant, oil resistant, medium resistant and other sealing aspects, such as hydraulic systems, lubrication systems, bearings and transmission devices of various machines. The second is to manufacture various hoses, such as aircraft oil pipelines, hot air ducts, high temperature and high pressure liquid hoses, etc.

[0004] However, due to the presence of fluorine atoms, the flexibility of the entire macromolecular chain of fluororubber is reduced, the rigidity is increased, and the resistance to molecular chain movement is large, so the cold resistance of fluororubber is poor. Among them, the brittle temperature of the standard sample 26 type fluororubber is -25 to -30°C, and the brittle temperature of 246 type fluororubber is -30 to -40°C. It can be seen that the cold resistance of type 26 fluororubber is worse than that of type 246 fluororubber. However, with the increasingly harsh use environment of sealing products, the performance requirements for fluororubber are also constantly improving, and its weakness of poor cold resistance is becoming increasingly prominent, which greatly limits its wide application. In order to promote the development of domestic sealing industry and broaden the application field of fluororubber, it is of practical significance to improve the cold resistance of fluororubber, especially type 26 fluororubber. Summary of the invention

[0005] The purpose of the present invention is to provide a low-temperature resistant modified binary fluororubber compound and a preparation method and use thereof.

[0006] The present invention provides a modified binary fluororubber compound, which is prepared from raw materials in the following weight ratio:

[0007] 100 parts of fluororubber, 1-5 parts of vulcanizing agent, 5-10 parts of acid absorbent, 10-30 parts of filler, 1-5 parts of processing aid, and 5-10 parts of white carbon black.

[0008] Furthermore, the aforementioned modified binary fluororubber compound is prepared from raw materials in the following weight ratio:

[0009] 100 parts of fluororubber, 2 parts of vulcanizing agent, 9 parts of acid absorber, 15 parts of filler, 2 parts of processing aid, and 5-10 parts of white carbon black.

[0010] Furthermore, the fluororubber is type 26 fluororubber.

[0011] Furthermore, the aforementioned modified binary fluororubber compound is prepared from raw materials in the following weight ratio:

[0012] 100 parts of 26 type fluororubber, 1-5 parts of vulcanizing agent, 5-10 parts of acid absorbent, 10-30 parts of filler, 1-5 parts of processing aid, 5-10 parts of white carbon black;

[0013] Preferably, it is prepared from raw materials in the following weight ratio:

[0014] 100 parts of 26 type fluororubber, 2 parts of vulcanizing agent, 9 parts of acid absorber, 15 parts of filler, 2 parts of processing aid, and 5-10 parts of white carbon black.

[0015] Furthermore, the raw material also includes a pigment, and the weight ratio of the pigment is 1-5 parts;

[0016] Preferably, the weight ratio of the pigment is 2 parts.

[0017] Further,

[0018] The acid absorber is composed of magnesium oxide and calcium hydroxide;

[0019] And / or, the filler is diatomaceous earth or carbon black;

[0020] Preferably, the mass ratio of magnesium oxide to calcium hydroxide is 3:6.

[0021] Furthermore, the aforementioned modified binary fluororubber compound is prepared from the following raw materials in the following weight ratio:

[0022] 100 parts of 26 type fluororubber, 1-5 parts of vulcanizing agent, 1-3 parts of magnesium oxide, 4-7 parts of calcium hydroxide, 10-30 parts of diatomaceous earth, 1-5 parts of processing aid, 1-5 parts of pigment, 5-10 parts of white carbon black;

[0023] Alternatively, it is prepared from the following raw materials in the following weight ratio:

[0024] 100 parts of 26 type fluororubber, 1-5 parts of vulcanizing agent, 1-3 parts of magnesium oxide, 4-7 parts of calcium hydroxide, 10-30 parts of carbon black, 1-5 parts of processing aid, and 5-10 parts of white carbon black.

[0025] Furthermore, the aforementioned modified binary fluororubber compound is prepared from the following raw materials in the following weight ratio:

[0026] 100 parts of 26 type fluororubber, 2 parts of vulcanizing agent, 3 parts of magnesium oxide, 6 parts of calcium hydroxide, 15 parts of diatomaceous earth, 2 parts of processing aid, 2 parts of pigment, 5 parts of white carbon black;

[0027] Alternatively, it is prepared from the following raw materials in the following weight ratio:

[0028] 100 parts of 26 type fluororubber, 2 parts of vulcanizing agent, 3 parts of magnesium oxide, 6 parts of calcium hydroxide, 15 parts of carbon black, 2 parts of processing aid, 5-10 parts of white carbon black;

[0029] Preferably,

[0030] The vulcanizing agent is Fluorine No. 5;

[0031] And / or, the processing aid is palm wax;

[0032] And / or, the pigment is iron red, phthalocyanine blue, phthalocyanine green or chromium oxide green.

[0033] The present invention also provides a method for preparing the aforementioned modified binary fluororubber compound, which comprises the following steps:

[0034] (1) Mixing fluororubber;

[0035] (2) Add other raw materials in turn and mix into agglomerates;

[0036] (3) Thinly pass the agglomerated product to obtain;

[0037] Preferably,

[0038] In step (1), the mixing temperature is 80-115° C.;

[0039] And / or, in step (1), the mixing time is 180-600 seconds;

[0040] And / or, in step (2), the mixing temperature is 80-115°C;

[0041] And / or, in step (2), the mixing time is 180-600 seconds;

[0042] And / or, in step (3), the thin pass is 3-8 times;

[0043] And / or, in step (3), the thin-pass temperature is 60-100°C.

[0044] The present invention also provides the use of the modified binary fluororubber compound in preparing seals, gaskets, spacers, diaphragms, hoses, oil seals, linings, anti-corrosion products, and electrical insulation products.

[0045] Compared with the prior art, the advantages of the present invention are:

[0046] The present invention provides a modified binary fluororubber compound. The modified binary fluororubber compound prepared by the present invention significantly reduces the low-temperature brittle temperature of the 26-type fluororubber while maintaining the good hardness and mechanical properties of the 26-type fluororubber, so that the low-temperature brittle temperature can reach below -35°C, and the low-temperature resistance effect is significantly improved. The modified fluororubber compound of the present invention has good hardness, mechanical properties and low-temperature resistance at the same time, and has excellent comprehensive performance, which can greatly expand the application of the 26-type fluororubber. At the same time, the present invention can greatly reduce production costs and improve production efficiency in practical applications, and has good application prospects.

[0047] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.

[0048] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. DETAILED DESCRIPTION

[0049] The raw materials and equipment used in the specific embodiments of the present invention are all known products and are obtained by purchasing commercially available products.

[0050] Example 1. Preparation of modified binary fluororubber compound of the present invention

[0051] 1. Raw materials

[0052] 100g of type 26 fluororubber, 2g of vulcanizing agent Fluorine-Linked No. 5, 3g of acid absorbent magnesium oxide and 6g of calcium hydroxide, 15g of diatomaceous earth, 2g of processing aid palm wax, 2g of pigment iron red, and 5g of white carbon black.

[0053] 2. Preparation method

[0054] Add 26 type fluororubber to the internal mixer and mix at 80℃ for 200 seconds. Then add vulcanizer, acid absorber, diatomaceous earth, processing aid, pigment and white carbon black in turn, mix into a mass, control the temperature at 80-90℃, and mix for 200-300s. Then pour it into the open mixer and pass it through 5 times to make a sheet. After 8-16 hours, pour it into the open mixer again and pass it through 5 times to make a sheet. The temperature of the open mixer is 60-70℃, and the modified binary fluororubber compound is obtained.

[0055] Example 2: Preparation of modified binary fluororubber compound of the present invention

[0056] 1. Raw materials

[0057] 100g of type 26 fluororubber, 2g of vulcanizing agent Fluorine-Linked No. 5, 3g of acid absorbent magnesium oxide and 6g of calcium hydroxide, 15g of carbon black, 2g of processing aid palm wax, and 5g of white carbon black.

[0058] 2. Preparation method

[0059] Add 26 type fluororubber into internal mixer and mix at 80℃ for 200 seconds. Then add vulcanizer, acid absorber, carbon black, processing aid and white carbon black in turn, mix into a mass, control the temperature at 80-90℃, mix for 200-300s, then pour into open mixer and pass through 5 times to produce sheets, stop for 8-16 hours, pour into open mixer again and pass through 5 times to produce sheets, the temperature of the open mixer is 60-70℃, and the modified binary fluororubber compound is obtained.

[0060] Example 3: Preparation of modified binary fluororubber compound of the present invention

[0061] 1. Raw materials

[0062] 100g of type 26 fluororubber, 2g of vulcanizing agent Fluorine-Linked No. 5, 3g of acid absorbent magnesium oxide and 6g of calcium hydroxide, 15g of carbon black, 2g of processing aid palm wax, and 7.5g of white carbon black.

[0063] 2. Preparation method

[0064] Add 26 type fluororubber into internal mixer and mix at 80℃ for 200 seconds. Then add vulcanizer, acid absorber, carbon black, processing aid and white carbon black in turn, mix into a mass, control the temperature at 80-90℃, mix for 200-300s, then pour into open mixer and pass through 5 times to produce sheets, stop for 8-16 hours, pour into open mixer again and pass through 5 times to produce sheets, the temperature of the open mixer is 60-70℃, and the modified binary fluororubber compound is obtained.

[0065] Example 4: Preparation of modified binary fluororubber compound of the present invention

[0066] 1. Raw materials

[0067] 100g of type 26 fluororubber, 2g of vulcanizing agent Fluorine-Linked No. 5, 3g of acid absorbent magnesium oxide and 6g of calcium hydroxide, 15g of carbon black, 2g of processing aid palm wax, and 10g of white carbon black.

[0068] 2. Preparation method

[0069] Add 26 type fluororubber into internal mixer and mix at 80℃ for 200 seconds. Then add vulcanizer, acid absorber, carbon black, processing aid and white carbon black in turn, mix into a mass, control the temperature at 80-90℃, mix for 200-300s, then pour into open mixer and pass through 5 times to produce sheets, stop for 8-16 hours, pour into open mixer again and pass through 5 times to produce sheets, the temperature of the open mixer is 60-70℃, and the modified binary fluororubber compound is obtained.

[0070] Comparative Example 1: Preparation of other modified binary fluororubber compounds

[0071] 1. Raw materials

[0072] 100g of type 26 fluororubber, 2g of vulcanizing agent Fluorine No. 5, 3g of acid absorbent magnesium oxide and 6g of calcium hydroxide, 15g of diatomaceous earth, 2g of processing aid palm wax, and 2g of pigment iron red.

[0073] 2. Preparation method

[0074] Add 26 type fluororubber into internal mixer and mix at 80℃ for 200 seconds. Then add vulcanizer, acid absorber, diatomaceous earth, processing aid and pigment in turn, mix into a mass, control the temperature at 80-90℃, mix for 200-300s, then pour into open mixer and pass through 5 times to produce sheets, stop for 8-16 hours, pour into open mixer again and pass through 5 times to produce sheets, the temperature of the open mixer is 60-70℃, and the modified binary fluororubber compound is obtained.

[0075] Comparative Example 2: Preparation of other modified binary fluororubber compounds

[0076] 1. Raw materials

[0077] 100g of type 26 fluororubber, 2g of vulcanizing agent Fluorine No. 5, 3g of acid absorbent magnesium oxide and 6g of calcium hydroxide, 15g of carbon black, and 2g of processing aid palm wax.

[0078] 2. Preparation method

[0079] Add 26 type fluororubber into internal mixer and mix at 80℃ for 200 seconds. Then add vulcanizer, acid absorber, carbon black and processing aid in sequence, mix into a mass, control the temperature at 80-90℃, mix for 200-300s, then pour into open mixer and pass through 5 times to produce sheets, stop for 8-16 hours, pour into open mixer again and pass through 5 times to produce sheets, the temperature of the open mixer is 60-70℃, and the modified binary fluororubber compound is obtained.

[0080] The beneficial effects of the present invention are demonstrated below through specific test examples.

[0081] Test Example 1: Study on the physical and chemical properties of the modified binary fluororubber compound of the present invention

[0082] 1. Experimental methods

[0083] The invention detects the hardness, tensile strength and low-temperature brittle temperature of the modified binary fluororubber compound. The hardness is detected according to the national standard GB / T 531.1-2008 method; the tensile strength is detected according to the national standard GB / T528-2009 method; and the low-temperature brittle temperature is detected according to the national standard GB / T 15256-2014 method.

[0084] 2. Experimental results

[0085] The results of the study on the physical and chemical properties of the modified binary fluororubber compound of the present invention are shown in Table 1.

[0086] Table 1. Study results of physical and chemical properties of binary fluororubber compound of the present invention

[0087]

[0088] According to the results in Table 1 above, the binary fluororubber mixes prepared in Examples 1 to 4 have good hardness, mechanical properties and low temperature resistance. Compared with the binary fluororubber mixes prepared in the comparative example, the binary fluororubber mixes prepared in Examples 1 to 4 have similar or better hardness and mechanical properties, while the low temperature brittle temperature is significantly reduced to below -35°C, which is equivalent to the low temperature brittle temperature of 246 type fluororubber, indicating that the low temperature resistance of the modified 26 type fluororubber is significantly improved. The modified 26 type fluororubber of the present invention not only maintains the original good hardness and mechanical properties, but also significantly improves the low temperature resistance, which is conducive to expanding the application range of 26 type fluororubber.

[0089] In summary, the present invention provides a modified binary fluororubber compound. The modified binary fluororubber compound prepared by the present invention significantly reduces the low-temperature brittle temperature of type 26 fluororubber while maintaining the good hardness and mechanical properties of type 26 fluororubber, so that its low-temperature brittle temperature can reach below -35°C, and the low-temperature resistance effect is significantly improved. The modified fluororubber compound of the present invention has good hardness, mechanical properties and low-temperature resistance at the same time, and has excellent comprehensive performance, which can greatly expand the application of type 26 fluororubber. At the same time, the present invention can greatly reduce production costs and improve production efficiency in practical applications, and has good application prospects.

Claims

1. A method for modifying the low temperature resistance of binary fluororubber compound. Features: The low temperature resistant modified binary fluororubber compound is prepared from the following raw materials in weight ratio: 100 parts of 26 type fluororubber, 1-5 parts of vulcanizing agent, 5-10 parts of acid absorbent, 10-30 parts of filler, 1-5 parts of processing aid, 5-10 parts of white carbon black; the acid absorbent is composed of magnesium oxide and calcium hydroxide; the filler is diatomaceous earth; the vulcanizing agent is Fluorine No. 5; the processing aid is palm wax; The method comprises the following steps: (1) Mixing fluororubber; (2) Add other raw materials in sequence and mix into agglomerates; (3) Thinly pass the agglomerated product through a tube.

2. The method according to claim 1, Features: The mass ratio of the magnesium oxide to calcium hydroxide is 3:

6.

3. The method according to claim 1, Features: The low temperature resistant modified binary fluororubber compound is prepared from the following raw materials in weight ratio: 100 parts of 26 type fluororubber, 2 parts of vulcanizing agent, 9 parts of acid absorber, 15 parts of filler, 2 parts of processing aid, and 5-10 parts of white carbon black.

4. The method according to claim 1, Features: The raw materials also include pigments, and the weight ratio of the pigments is 1-5 parts.

5. The method according to claim 4, Features: The weight ratio of the pigment is 2 parts.

6. The method according to claim 1, Features: The low temperature resistant modified binary fluororubber compound is prepared from the following raw materials in weight ratio: 100 parts of 26 type fluororubber, 1-5 parts of vulcanizing agent, 1-3 parts of magnesium oxide, 4-7 parts of calcium hydroxide, 10-30 parts of diatomaceous earth, 1-5 parts of processing aid, 1-5 parts of pigment, and 5-10 parts of white carbon black.

7. The method according to claim 6, Features: The low temperature resistant modified binary fluororubber compound is prepared from the following raw materials in weight ratio: 100 parts of 26 type fluororubber, 2 parts of vulcanizing agent, 3 parts of magnesium oxide, 6 parts of calcium hydroxide, 15 parts of diatomaceous earth, 2 parts of processing aid, 2 parts of pigment, and 5 parts of white carbon black.

8. The method according to claim 7, Features: The pigment is iron red, phthalocyanine blue, phthalocyanine green or chromium oxide green.

9. The method according to claim 1, Features: In step (1), the mixing temperature is 80-115°C; And / or, in step (1), the mixing time is 180-600 seconds; And / or, in step (2), the mixing temperature is 80-115°C; And / or, in step (2), the mixing time is 180-600 seconds; And / or, in step (3), the thin pass is performed 3-8 times; And / or, in step (3), the thin pass temperature is 60-100°C.

10. Use of the low-temperature resistant modified binary fluororubber compound prepared by the method according to any one of claims 1 to 9 in the preparation of seals, gaskets, spacers, diaphragms, hoses, oil seals, linings, anti-corrosion products, and electrical insulation products.