A composite rubber lining and its preparation method and application
By adopting composite structure and specific formula components in the rubber lining, the problems of insufficient bonding strength and poor aging resistance in the prior art are solved, and high bonding strength and aging resistance are achieved, which is suitable for ore dressing equipment. Field application.
Patent Information
- Application Number
- CN202211445731.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-18
AI Technical Summary
The bonding strength of the existing pre-vulcanized wear-resistant rubber lining and room temperature curing adhesive is insufficient, and the aging resistance is poor, especially in the on-site lining application of ore dressing equipment.
The composite rubber lining structure is adopted, including a wear-resistant layer and an adhesive layer. The wear-resistant layer is composed of natural rubber and butyl rubber. The thickness of the adhesive layer is 0.6-1.2mm, and the roughness formed by the printed fabric on the surface is 60-110μm. No need for grinding after vulcanization, combined with specific formula components such as paraffin, nano zinc oxide and phenolic resins, enhance bond strength and aging resistance.
It achieves high bond strength and aging resistance, simplifies the construction process, improves construction efficiency, and avoids the necessity of bonding surface polishing. It is suitable for use in high wear and high corrosion resistance ore dressing equipment.
Smart Images

Figure BDA0003949559930000051 
Figure BDA0003949559930000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber linings, and in particular to a composite rubber lining and a preparation method and application thereof. Background Art
[0002] Under the trend of green and low-carbon development, the new energy industry chain has ushered in unprecedented development opportunities, and the demand for related mineral resources has increased dramatically, which has effectively promoted the development and application of various new, efficient and large-scale mineral processing equipment. Lining the inner surface of mineral processing equipment with one or more layers of anti-corrosion and wear-resistant rubber lining is the most effective way to extend the service life of the equipment. The above equipment requires rubber linings with high wear resistance, high aging resistance, high bonding strength and high corrosion resistance, especially pre-vulcanized wear-resistant linings suitable for on-site rubber lining.
[0003] The existing wear-resistant rubber is mainly a combination of natural rubber and carbon black, and the pre-vulcanized rubber sheet has a very unsatisfactory light aging resistance, and the surface thereof usually needs to be polished before bonding in order to have a good bonding strength with the room temperature curing adhesive. Therefore, in order to solve the above problems existing in the prior art, the present invention is hereby provided. Summary of the invention
[0004] In view of at least one of the above-mentioned problems existing in the prior art, the present invention provides a composite rubber lining and a preparation method and application thereof, aiming to solve the problems of insufficient bonding strength between the existing pre-vulcanized wear-resistant rubber lining and the room temperature curing adhesive and poor aging resistance.
[0005] To achieve the above objectives, one of the objectives of the present invention is to provide a composite rubber lining, comprising a wear-resistant layer and a bonding layer;
[0006] The wear-resistant layer is compounded of natural rubber and butadiene rubber;
[0007] The thickness of the bonding layer is 0.6-1.2 mm, the side of the bonding layer facing away from the wear-resistant layer is a bonding surface, the bonding surface is printed with cloth texture, and the surface roughness formed by the cloth texture is 60-110 μm;
[0008] The composite rubber lining does not need to be polished after vulcanization. Compared with the rubber lining in the prior art, the rubber lining of the present invention is a composite structural layer, and the bonding surface is printed with cloth texture. The roughness formed by the cloth texture is about 60-110μm, so that the bonding layer does not need to be polished, and it can have good anchoring bonding strength with the room temperature curing adhesive, which is particularly suitable for on-site rubber lining of anti-corrosion and wear-resistant equipment such as mineral processing equipment. It should be noted that the formation of the surface roughness of the bonding layer in the present invention can be formed by printing the texture on the isolation cloth rolled together with the composite rubber sheet on the bonding surface of the bonding layer after vulcanization during the winding process of the composite rubber sheet. The surface roughness formed by the cloth texture is 60-110μm. If the roughness is too small, it is not conducive to forming a firm anchoring, and the bonding force is low; if the roughness is too large, the bonding surface is not tightly fitted, which will also reduce the bonding strength. Therefore, it is necessary to select an isolation cloth with appropriate textures to form the required roughness on the bonding surface of the bonding layer.
[0009] Preferably, the wear-resistant layer comprises the following components in parts by weight: 50-100 parts of natural rubber, 0-50 parts of cis-1,4-butadiene rubber, 20-40 parts of high wear-resistant carbon black, 0-20 parts of silicon powder, 1-2 parts of Rhine powder 42M, 5-10 parts of nano zinc oxide, 3-6 parts of antioxidant composition, 1.6-2.0 parts of sulfur, and 0.4-1.0 parts of accelerator CZ. The use of cis-1,4-butadiene rubber in natural rubber and the reasonable control of the ratio of the two are helpful to improve the wear resistance and resilience of the lining. Preferably, the antioxidant composition comprises the following components in parts by weight: 1-2 parts of antioxidant RD, 1-2 parts of antioxidant 4010NA and 1.5-2 parts of paraffin. The number of paraffin wax is as high as 1.5-2.0 parts, which is particularly beneficial to improve the light aging resistance of the lining. In the existing pre-vulcanized wear-resistant natural rubber lining without a composite layer, if the weight of paraffin wax exceeds 1 part, the bonding strength is usually significantly reduced. The paraffin content in the composite rubber lining of the present invention exceeds 1 part. Since the composite layer (adhesive layer) blocks the paraffin in the wear-resistant layer from migrating to the adhesive, the problem of increasing the amount of paraffin, which is unfavorable to the bonding strength, is solved. Rhine powder 42M is an anhydrous mixture of fatty alcohols and fatty acids. It is an excellent filler and chemical dispersant. It helps to improve the uniformity of the distribution of each component in the wear-resistant layer, improve the plasticity of the raw rubber, and improve fluidity. Silica powder has good wear resistance and excellent electrical insulation. It is evenly dispersed in the rubber lining, which can improve the surface resistance of the lining, offset the conductivity that may be caused by high-wear-resistant carbon black, and help the lining to detect defects such as pinholes with a high-frequency spark tester. Compared with ordinary zinc oxide, nano zinc oxide is beneficial to improve the aging resistance and wear resistance of wear-resistant rubber.
[0010] Preferably, the bonding layer comprises the following components in parts by weight: 30-50 parts of chloroprene rubber, 50-70 parts of natural rubber, 20-25 parts of clay, 20-30 parts of talc, 20-25 parts of barium sulfate, 2.0-3.0 parts of magnesium oxide, 3.0-5.0 parts of zinc oxide, 1.0-1.4 parts of sulfur, 0.5-0.6 parts of accelerator CZ, and 0.2-0.4 parts of accelerator TMTD. Natural rubber is conducive to the bonding of the bonding layer with the wear-resistant layer, and chloroprene rubber is particularly conducive to the bonding of the bonding layer with the room temperature curing adhesive. Further preferably, the bonding layer also comprises the following components in parts by weight: 3-6 parts of phenolic resin. Phenolic resin has good compatibility with both natural rubber and chloroprene rubber, is conducive to improving the dispersion uniformity of natural rubber and chloroprene rubber, helps to improve the bonding of the bonding layer with the wear-resistant layer, and also helps to improve the bonding of the bonding layer with the adhesive.
[0011] Another object of the present invention is to provide a method for preparing a composite rubber lining, comprising the following steps:
[0012] Step 1, weighing each component according to the weight of each component in the bonding layer formula, preparing the bonding layer rubber material, putting it into a banbury mixer for 5-10 minutes to make a mixed rubber, and then pressing it into sheets through an open mixer, and then cutting it into strips of rubber material, cooling it through a film cooler and air-drying it for standby use, and then extruding a rubber sheet of about 0.6-1.2 mm through an extruder, and rolling the rubber sheet and the isolation film or isolation cloth together on a roller through a winder to form a bonding layer rubber sheet for standby use;
[0013] Step 2, weighing each component according to the weight of each component in the wear-resistant layer formula, preparing the wear-resistant layer rubber material, putting it into a banbury mixer for 5-10 minutes to make a mixed rubber, and then pressing it into sheets through an open mixer, and then cutting it into strips of rubber material, cooling it through a film cooler and air-drying it for standby use;
[0014] Step 3, hanging the adhesive layer rubber sheet obtained in step 1 above the conveyor belt of the extruder;
[0015] Step 4, extruding the mixed rubber obtained in step 2 into a wear-resistant rubber sheet with a thickness of 2.5 to 7 mm on an extruder, and the wear-resistant rubber sheet moves toward the winding roller along the conveyor belt;
[0016] At this time, the adhesive layer rubber sheet hanging above the conveyor belt is unwound, and the adhesive layer rubber sheet is introduced onto the conveyor belt through the guide roller, and adhered to the wear-resistant layer rubber sheet, and then tightly adhered together by the pressing roller to form a composite rubber sheet, and then continues to move to the winding roller, and the composite rubber sheet and the isolation cloth with specific patterns are rolled on the roller together;
[0017] Step 5, the composite rubber sheet obtained in step 4 is moved to a vulcanization tank for vulcanization. The specific vulcanization conditions are: pressure of 0.3-0.6 MPa, heating to 125-135° C., vulcanization for 6-10 hours, stopping heating, maintaining the pressure above 0.15 MPa, cooling to 60° C., ending the vulcanization, opening the vulcanization tank door, and after the composite rubber sheet is completely cooled, unwinding and removing the isolation cloth to obtain a pre-vulcanized composite rubber lining, wherein the surface of the bonding layer is printed with cloth texture and the roughness is about 60-110 μm.
[0018] Another object of the present invention is to provide the use of the composite rubber lining described above or the composite rubber lining prepared by the above preparation method in mineral processing equipment.
[0019] Preferably, the construction process of the composite rubber lining includes the following steps:
[0020] (1) The parts of the equipment that need rubber lining are sandblasted to Sa2.5, and then the SP-1 primer is applied. After air drying, the first coat of SP-1 adhesive is applied. After air drying, the second coat of SP-1 adhesive is applied to obtain the base body;
[0021] (2) Cut the composite rubber lining according to the surface shape and size of the lined equipment, apply the first coat of SP-1 adhesive on the bonding surface, apply the second coat of SP-1 adhesive after air drying, and air dry to obtain the rubber sheet;
[0022] (3) laying the obtained rubber sheet on the obtained substrate, and pressing the rubber sheet with a pressure roller to closely adhere the rubber sheet to the substrate;
[0023] (4) At room temperature of 23°C, the adhesive is fully cured after 48 hours.
[0024] Compared with the prior art, the advantages of the present invention are:
[0025] The composite rubber lining of the present invention solves the problem of insufficient bonding strength between the pre-vulcanized wear-resistant natural rubber lining and the room temperature curing adhesive, and also solves the problem that the antioxidant in the natural rubber migrates to the adhesive to affect its bonding strength. The dosage of the antioxidant is optimized, thereby improving the aging resistance of the lining. The present invention prints the texture of the isolation cloth on the adhesive layer to form a grid texture surface with a roughness of about 60 to 110 μm. Such roughness is particularly conducive to the formation of an anchoring structure between the lining and the adhesive, and is conducive to improving the bonding strength. Compared with the existing pre-vulcanized rubber lining, the lining of the present invention does not need to be polished, has a very high bonding strength, improves the construction environment, and improves the construction efficiency. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0027] A composite rubber lining provided in an embodiment of the present invention comprises a wear-resistant layer and an adhesive layer. The wear-resistant layer is composited with natural rubber and butadiene rubber; the thickness of the adhesive layer is 0.6-1.2 mm, the side of the adhesive layer facing away from the wear-resistant layer is the adhesive surface, the adhesive surface is printed with cloth texture, and the surface roughness formed by the cloth texture is 60-110 μm; the composite rubber lining does not need to be polished after vulcanization.
[0028] A method for preparing a composite rubber lining provided in an embodiment of the present invention comprises the following steps:
[0029] Step 1, weighing each component according to the weight of each component in the bonding layer formula, preparing the bonding layer rubber material, putting it into a banbury mixer for 5-10 minutes to make a mixed rubber, and then pressing it into sheets through an open mixer, and then cutting it into strips of rubber material, cooling it through a film cooler and air-drying it for standby use, and then extruding a rubber sheet of about 0.6-1.2 mm through an extruder, and rolling the rubber sheet and the isolation film or isolation cloth together on a roller through a winder to form a bonding layer rubber sheet for standby use;
[0030] Step 2, weighing each component according to the weight of each component in the wear-resistant layer formula, preparing the wear-resistant layer rubber material, putting it into a banbury mixer for 5-10 minutes to make a mixed rubber, and then pressing it into sheets through an open mixer, and then cutting it into strips of rubber material, cooling it through a film cooler and air-drying it for standby use;
[0031] Step 3, hanging the adhesive layer rubber sheet obtained in step 1 above the conveyor belt of the extruder;
[0032] Step 4: Extrude the mixed rubber obtained in step 2 into a wear-resistant rubber sheet with a thickness of 2.5 to 7 mm on an extruder, and the wear-resistant rubber sheet moves toward the winding roller along the conveyor belt.
[0033] At this time, the adhesive layer rubber sheet hanging above the conveyor belt is unwound, and the adhesive layer rubber sheet is introduced onto the conveyor belt through the guide roller, and adhered to the wear-resistant layer rubber sheet, and then tightly adhered together by the pressing roller to form a composite rubber sheet, and then continues to move to the winding roller, and the composite rubber sheet and the isolation cloth with specific patterns are rolled on the roller together;
[0034] Step 5, the composite rubber sheet obtained in step 4 is moved to a vulcanization tank for vulcanization. The specific vulcanization conditions are: pressure of 0.3-0.6 MPa, heating to 125-135° C., vulcanization for 6-10 hours, stopping heating, maintaining the pressure above 0.15 MPa, cooling to 60° C., ending the vulcanization, opening the vulcanization tank door, and after the composite rubber sheet is completely cooled, unwinding and removing the isolation cloth to obtain a pre-vulcanized composite rubber lining, wherein the surface of the bonding layer is printed with cloth texture and the roughness is about 60-110 μm.
[0035] Table 1 Component ratio of the composite rubber lining of the present invention and the wear-resistant natural rubber commonly used in the market
[0036]
[0037]
[0038] The finished products of Examples 1 to 6 are composite rubber linings respectively prepared by using the composition ratio of the wear-resistant layer and the adhesive layer of the present invention and the preparation process of the present invention. Examples 7 to 9 are wear-resistant layer rubber sheets (i.e., rubber sheets without adhesive layers) respectively prepared by using the composition ratio of the wear-resistant layer of the present invention and the preparation process of the wear-resistant layer rubber sheet in the preparation process of the present invention. Comparative Examples 1 to 4 are composite rubber sheets respectively prepared by roller bonding the wear-resistant natural rubber commonly used in the market and the adhesive layer rubber sheet 1 and the adhesive layer rubber sheet 2 prepared by the preparation process of the present invention. Comparative Examples 5 to 6 are respectively ordinary rubber sheets prepared by using the wear-resistant natural rubber commonly used in the market and the preparation method of the wear-resistant layer rubber sheet of the present invention.
[0039] The thickness of the wear-resistant rubber sheet 1, the wear-resistant rubber sheet 2, the wear-resistant rubber sheet 3 and the thickness of the ordinary rubber sheet 1, the ordinary rubber sheet 2 are all 5 mm. The thickness of the adhesive layer rubber sheet 1, the adhesive layer rubber sheet 2, the adhesive layer rubber sheet 3 are all 1 mm.
[0040] The prepared ordinary rubber sheet 1, ordinary rubber sheet 2 and wear-resistant layer rubber sheet 1, wear-resistant layer rubber sheet 2, wear-resistant layer rubber sheet 3 are pasted on the steel plate according to the above-mentioned construction process of the composite rubber lining. After 48 hours at room temperature, the 90° peeling strength is tested to be 2.4N / mm, 2.8N / mm, 2.0N / mm, 2.2N / mm, and 2.6N / mm respectively. The peeling state is: the adhesive is peeled off from the wear-resistant layer rubber sheet or the ordinary rubber sheet. This also indicates that the adhesive is not sufficiently bonded to the wear-resistant layer rubber sheet and the ordinary rubber sheet. For the above-mentioned wear-resistant layer rubber sheet and ordinary rubber sheet, the bonding surface is usually polished with a grinder at the construction site to improve the surface roughness, and then pasted to the equipment according to the above-mentioned construction process steps. The bonding force can reach 2.8N / mm to 6.0N / mm. The peeling state is still that the adhesive is peeled off from the surface of the rubber sheet, and the bonding force is still insufficient. In addition, on-site polishing consumes a lot of manpower, and the dust generated by polishing affects the working environment.
[0041] The prepared composite rubber lining 1, composite rubber lining 2, composite rubber lining 3, composite rubber lining 4, composite rubber lining 5, and composite rubber lining 6 were pasted on the steel plate according to the above-mentioned construction process steps of the composite rubber lining. After 48 hours at room temperature, the 90° peeling strength was tested. The peeling strength was 6.2N / mm~9.0N / mm, and the peeling state was: rupture in the bonding layer. This shows that the bonding force between the bonding layer rubber sheet and the room temperature curing adhesive is greater than the cohesive force of the bonding layer rubber sheet, which well solves the problem of insufficient bonding strength between the single-layer rubber lining (that is, the rubber lining containing only the wear-resistant layer) and the room temperature curing agent in the prior art.
[0042] The prepared composite rubber sheets 1, 2, 3 and 4 were bonded to the steel plates according to the construction process of the composite rubber lining. After 48 hours at room temperature, the 90° peel strength was tested, which was also between 6.2 N / mm and 9.0 N / mm. The peeling state was: rupture within the adhesive layer.
[0043] The prepared composite rubber lining 1, composite rubber lining 2, composite rubber lining 3, composite rubber lining 4, composite rubber lining 5, composite rubber lining 6 and composite rubber sheet 1, composite rubber sheet 2, composite rubber sheet 3, composite rubber sheet 4 were respectively pasted on the channel steel and placed in a sunny place to observe the changes in the rubber surface, especially the changes in the positive corner. The results are as follows: composite rubber sheet 1 and composite rubber sheet 3 were exposed to the sun for 4 weeks in summer, and there was no obvious change on the flat rubber surface, but slight cracks appeared in the positive corner, and the degree of cracks increased with the increase of exposure time; composite rubber sheet 2 and composite rubber sheet 4 were exposed to the sun for 6 weeks in summer, and slight cracks appeared in the positive corner, and the degree of cracks increased with the increase of exposure time. Composite rubber lining 1, composite rubber lining 2, composite rubber lining 3, composite rubber lining 4, composite rubber lining 5, composite rubber lining 6 were exposed to the sun for 12 weeks in summer, and no cracks appeared in the positive corner. This shows that the light aging resistance of composite rubber lining 1, composite rubber lining 2, composite rubber lining 3, composite rubber lining 4, composite rubber lining 5, and composite rubber lining 6 is obviously better than that of composite rubber plate 1, composite rubber plate 2, composite rubber plate 3, and composite rubber plate 4, that is, the light aging resistance of the composite rubber lining obtained by the formula and preparation process of the present invention is obviously better than the existing pre-vulcanized wear-resistant rubber lining on the market.
[0044] It should be emphasized that the above are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.
[0045] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A composite rubber lining, characterized in that: comprising a wear-resistant layer and a bonding layer; The wear-resistant layer is compounded of natural rubber and butadiene rubber; The thickness of the bonding layer is 0.6-1.2 mm, the side of the bonding layer facing away from the wear-resistant layer is a bonding surface, the bonding surface is printed with cloth texture, and the surface roughness formed by the cloth texture is 60-110 μm; The composite rubber lining does not need to be polished after vulcanization; The wear-resistant layer comprises the following components in parts by weight: 50-100 parts of natural rubber, 30-50 parts of butadiene rubber, 20-45 parts of high wear-resistant carbon black, 0-20 parts of silicon powder, 1-2 parts of Rheinland 42M, 5-10 parts of nano zinc oxide, 3-6 parts of antioxidant composition, 1.6-2.0 parts of sulfur, and 0.4-1.0 parts of accelerator CZ; The antioxidant composition comprises the following components in parts by weight: 1-2 parts of antioxidant RD, 1-2 parts of antioxidant 4010NA and 1.5-2 parts of paraffin; The bonding layer comprises the following components in parts by weight: 30-50 parts of chloroprene rubber, 50-70 parts of natural rubber, 20-25 parts of clay, 20-30 parts of talc, 20-25 parts of barium sulfate, 2.0-3.0 parts of magnesium oxide, 3.0-5.0 parts of zinc oxide, 1.0-1.4 parts of sulfur, 0.5-0.6 parts of accelerator CZ, and 0.2-0.4 parts of accelerator TMTD.
2. A composite rubber lining according to claim 1, characterized in that: The bonding layer further comprises the following components in parts by weight: 3 to 6 parts of phenolic resin.
3. A method for preparing a composite rubber lining, characterized in that: The composite rubber lining is the composite rubber lining according to any one of claims 1 to 2, and the preparation method comprises the following steps: Step 1, weighing each component according to the weight of each component in the bonding layer formula, preparing the bonding layer rubber material to make a mixed rubber, and then extruding a 0.6-1.2 mm bonding layer rubber sheet through an extruder, and rolling the bonding layer rubber sheet on a release film or a release cloth for standby use; Step 2, weighing each component according to the weight of each component in the wear-resistant layer formula, preparing the wear-resistant layer rubber material, and making a mixed rubber; Step 3, hanging the adhesive layer rubber sheet obtained in step 1 above the conveyor belt of the extruder; Step 4, the mixed rubber obtained in step 2 is extruded into a wear-resistant layer rubber sheet with a thickness of 2.5-7 mm on an extruder, and the wear-resistant layer rubber sheet moves toward a winding roller along with a conveyor belt. At this time, the adhesive layer rubber sheet suspended above the conveyor belt is unwound, and the adhesive layer rubber sheet is introduced onto the conveyor belt through a guide roller and adhered to the wear-resistant layer rubber sheet to form a composite rubber sheet, and then continues to move toward the winding roller, and the composite rubber sheet and the isolation cloth with specific patterns are rolled on the roller together; Step 5: Put the composite rubber sheet obtained in step 4 into a vulcanizer for vulcanization. After the vulcanization is completed, unwind it to obtain a pre-vulcanized composite rubber lining, in which the surface of the bonding layer is printed with cloth texture and the roughness is 60-110 μm.
4. The method for preparing a composite rubber lining according to claim 3, characterized in that: Use a three-roll calender instead of an extruder; or In step 4, the length of each roll of the composite rubber sheet is 7 to 20 meters.
5. Use of the composite rubber lining according to any one of claims 1 to 2 or the composite rubber lining prepared by the preparation method according to any one of claims 3 to 4 in mineral processing equipment.
6. The use of the composite rubber lining according to claim 5, characterized in that: The construction process of the composite rubber lining in the mineral processing equipment includes the following steps: (1) Sandblast the surface of the equipment to be lined with rubber to Sa2.5, clean it, apply SP-1 primer, air dry it, apply the first coat of SP-1 adhesive, and then air dry it, apply the second coat of SP-1 adhesive; (2) Clean the surface of the composite rubber lining, apply the first coat of SP-1 adhesive on the bonding surface of the bonding layer, and after air drying, apply the second coat of SP-1 adhesive, and air dry to obtain the rubber sheet; (3) Place the obtained rubber sheet on the equipment coated with SP-1 adhesive and press it with a pressure roller to press the composite rubber lining tightly onto the adhesive on the surface of the equipment; (4) After 48 hours at room temperature (23°C), the adhesive is fully cured.
7. The use of the composite rubber lining according to claim 6, characterized in that: The SP-1 adhesive is a room temperature curing chloroprene rubber adhesive.