Methods for preparing powder and coating for spraying
By optimizing atmospheric pressure plasma spraying conditions and ceramic particle composition, the problem of balancing the fluidity and density of the sprayed film was solved, achieving a higher quality spraying effect.
Patent Information
- Application Number
- CN202211217540.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-30
- Filing Date
- 2022-09-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-09-30
AI Technical Summary
It is difficult to achieve both fluidity and density in existing spray-coated films. In particular, the miniaturization of ceramic particles during the spray-coating process can reduce fluidity and affect the spray-coating effect.
By adjusting the spraying conditions during atmospheric pressure plasma spraying, including argon and helium pressure, plasma output, spraying speed and distance, the average particle size of the powder used for spraying is reduced, the composition and morphology of ceramic particles are optimized, and both fluidity and density are ensured.
This enables the supply of finer ceramic particles, resulting in a dense spray-coated film with low porosity and a flat surface, thus improving the stability and quality of the spray-coating process.
Smart Images

Figure CN115896672B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to powder for spray coating. Furthermore, this invention relates to a method for preparing a spray-coated film using the powder for spray coating. Background Technology
[0002] The technology of imparting new functions by covering the surface of a substrate with various materials has been used in various fields. As an example of this surface coating technology, a spray coating method is known, in which ceramic particles formed of ceramic are blown onto the surface of a substrate in a molten state, thereby forming a spray coating film formed of the ceramic.
[0003] For example, in the manufacturing of semiconductor devices, dry etching using plasmas containing halogen gases such as fluorine, chlorine, and bromine is sometimes used to perform micro-machining on the surface of semiconductor substrates. After dry etching, oxygen plasma is used to clean the interior of the chamber where the semiconductor substrate is removed. Within this chamber, components exposed to highly reactive oxygen plasma and halogen gas plasma will be corroded. Therefore, in semiconductor device manufacturing equipment, to prevent plasma-induced corrosion, a ceramic-coated film is applied to components exposed to plasmas such as oxygen and halogen gases.
[0004] In the spraying methods disclosed in Patent Documents 1-3, the powder material for spraying (spraying powder) is supplied to the spraying apparatus in a dry state. In order to stably supply the spraying powder to the spraying apparatus, the development of spraying powder with improved flowability is underway.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: Japanese Patent No. 6811188
[0008] Patent Document 2: Japanese Patent No. 4630799
[0009] Patent Document 3: Japanese Patent No. 6262716 Summary of the Invention
[0010] The problem the invention aims to solve
[0011] On the other hand, from the viewpoint of improving the durability of the sprayed film, it is desirable to form a sprayed film with a smoother surface and higher density. One method to improve the smoothness and density of the sprayed film is, for example, to further reduce the size of the ceramic particles constituting the spraying powder. However, simply reducing the size of the ceramic particles risks reducing the flowability of the spraying powder. Therefore, there is still room for improvement in the design of the ceramic particles.
[0012] In view of this situation, the object of the present invention is to provide a technique that maintains a flowability suitable for spraying and allows for the supply of finer ceramic particles to the workpiece (substrate) during spraying.
[0013] Solution for solving the problem
[0014] The inventors focused on the following: During the spraying of granulated sintered particles, the primary particles constituting the granulated sintered particles melt due to the heat energy during spraying and enter the gaps, thereby reducing the particle size. Furthermore, the inventors confirmed that in the sprayed film formed using granulated sintered particles, a portion of the sprayed granulated sintered particles directly reaches the substrate in an unmelted state and may remain in the sprayed film. Moreover, the inventors' in-depth research revealed that by intentionally increasing the gaps between the granulated sintered particles, the sprayed granulated sintered particles can be completely melted. Furthermore, the inventors discovered that a sprayed film can be produced by supplying the substrate with particles smaller than before, thus completing the present invention.
[0015] The spray-coating powder disclosed herein is composed of ceramic particles. The characteristic of this spray-coating powder is that...
[0016] When comparing the powder for spraying with the powder before and after atmospheric pressure plasma spraying in water under the following conditions, the average particle size (D) of the powder for spraying, based on laser diffraction scattering method, is as follows: 50 The value of ) should be reduced by at least 25%.
[0017] The conditions are as follows:
[0018] Plasma working gas:
[0019] Argon (Ar) gas: 50 psi; and
[0020] Helium (He): 50 psi
[0021] Plasma output: 36kW
[0022] Powder feed rate for spraying: 20g / min
[0023] Spraying distance: 400mm.
[0024] The powder used for spraying is composed of the following: heat energy generated during spraying, average particle size (D) 50 The particle size is reduced by at least 25% compared to before spraying. Therefore, during spraying, finer spraying powder can be supplied to the substrate. In addition, the particle size of the spraying powder can be set in a way that achieves a flowability suitable for spraying.
[0025] In a preferred embodiment, the stationary angle of the spray-coating powder disclosed herein is 40 degrees or less. The stationary angle of this spray-coating powder is set in a manner that achieves flowability suitable for spray coating.
[0026] Alternatively, another preferred embodiment of the spray-coating powder disclosed herein is composed of oxide ceramic particles. By using the spray-coating powder of this composition, a spray-coated film made of oxide ceramic can be produced.
[0027] In another preferred embodiment of the spray-plating powder disclosed herein, the ceramic particles are granulated and sintered particles formed from primary particles of the ceramic. Preferably, the average ratio of the area of openings on the surface of the ceramic particles, as observed by SEM, to the total surface area is 20% or more. In this configuration of the spray-plating powder, the proportion of the area of openings within the aforementioned range increases the degree of thermal shrinkage of the spray-plating powder. Therefore, during spray plating, finer spray-plating powder can be supplied to the substrate.
[0028] In another preferred embodiment of the spray-plating powder disclosed herein, the ceramic particles are granulated and sintered particles formed from primary particles of the ceramic, and when the surface of the ceramic particles is observed by SEM, the ratio (Dmax / Dmin) of the maximum diameter Dmax to the minimum diameter Dmin of the openings present on the surface is 1 to 1.8. The shape of the openings observed by SEM on the surface of the ceramic particles is as specified above for the spray-plating powder, and its thermal shrinkage is improved. Therefore, during spray plating, a finer spray-plating powder can be supplied to the substrate.
[0029] Furthermore, in another preferred embodiment of the spray-coating powder disclosed herein, the average particle size (D) of the aforementioned primary particles based on laser diffraction scattering method is... 50 The thickness is 0.5 μm or more and 5 μm or less. Based on this structure, the mixing of spraying powder containing unmelted portions into the sprayed film and the generation of defects in the sprayed film can be suppressed. Furthermore, a denser sprayed film can be produced.
[0030] Furthermore, in another preferred embodiment of the spray-plating powder disclosed herein, the bulk density is 1.0 or less. Due to this configuration, the micronization effect of the spray-plating powder based on spray plating is further improved.
[0031] Furthermore, based on the technology disclosed herein, a method for manufacturing a spray-coated film is disclosed. Specifically, a method is provided for spraying any of the spray-coating powders disclosed herein onto the surface of a substrate to be sprayed, thereby manufacturing a spray-coated film. In this method, during spraying, finer spray-coating powders are supplied to the substrate, thus, for example, it is suitable to manufacture a dense and flat spray-coated film with a porosity of 4% or less and a surface roughness (arithmetic mean roughness) Ra of 3.5 μm or less. Attached Figure Description
[0032] Figure 1 This is a schematic diagram illustrating an example of fabricating a sprayed film using the spraying powder in one embodiment.
[0033] Figure 2 This is a schematic diagram illustrating an example of fabricating a sprayed film using conventional spraying powder.
[0034] Figure 3 The image shows a SEM image of the surface of the sprayed powder in sample 1.
[0035] Figure 4 The image shows a cross-sectional SEM image of the sprayed powder of sample 1.
[0036] Figure 5 The image shows a SEM image of the surface of the sprayed powder in sample 2.
[0037] Figure 6 The image shows a cross-sectional SEM image of the sprayed powder of sample 2.
[0038] Figure 7 The image shows a SEM image of the surface of the sprayed powder in sample 3.
[0039] Figure 8 The image shows a cross-sectional SEM image of the sprayed powder of sample 3.
[0040] Figure 9 The image shows a SEM image of the flying particles from sample 1.
[0041] Figure 10 SEM images of the flying particles of sample 2.
[0042] Figure 11 SEM images of the flying particles in sample 3.
[0043] Figure 12 The image shows a cross-sectional SEM image of the sprayed film of sample 1.
[0044] Figure 13 The image shows a cross-sectional SEM image of the sprayed film of sample 2.
[0045] Figure 14 The image shows a cross-sectional SEM image of the sprayed film of sample 3.
[0046] Figure 15 A graph showing the surface roughness Ra (μm) of the sprayed films of samples 1-3.
[0047] Explanation of reference numerals in the attached figures
[0048] 11, 21 Ceramic Particles
[0049] 12, 22 flying particles
[0050] 23 Unmelted particles
[0051] L1 and L2 spray coatings
[0052] S substrate Detailed Implementation
[0053] The following describes suitable embodiments of the present invention. It should be noted that, for matters not specifically described in this specification but necessary for the implementation of the present invention, those skilled in the art can grasp them based on existing technology and conventional technical means. The present invention can be implemented based on the content disclosed in this specification and common technical knowledge in the field. It should be noted that, unless otherwise specified, the use of "X~Y" to indicate a numerical range in the specification means "above X and below Y," and it should be understood that this numerical range also includes the range "above X and below Y."
[0054] <Definition>
[0055] In this specification, "powder for spraying" refers to a powdered material used in spraying. The powder for spraying disclosed herein is a powder material for spraying that is substantially composed of ceramic particles and may contain unavoidable impurities other than the target ceramic particles (e.g., trace amounts of tiny non-ceramic particles).
[0056] In this specification, "primary particle" means the smallest unit of the morphological components constituting the above-described spray-coating powder that can be visually identified as a granular object. When the ceramic particles constituting the spray-coating powder disclosed herein include secondary particles (e.g., granulated particles), the particles constituting the secondary particles may also be referred to as primary particles.
[0057] Here, "secondary particles" refers to primary particles that are three-dimensionally combined to form a single granular material (exhibiting a granular morphology). Granulated particles and granulated-sintered particles after granulation are examples of "secondary particles" in this context. It should be noted that "combination" here refers to the direct or indirect combination of two or more primary particles, including: combination between primary particles based on chemical reactions; combination where primary particles attract each other simply through adsorption; combination using the anchoring effect of the unevenness of the primary particle surface to allow adhesive materials to enter; combination using the electrostatic attraction effect; and combination where the surfaces of primary particles melt and become integrated.
[0058] In addition, when "raw material particles" are mentioned in this specification, they refer to the particles that constitute the powder in the raw material stage used to make the spraying powder disclosed herein.
[0059] <Method for determining the average particle size of powders used in spraying>
[0060] In this specification, the term "average particle size (D)" is used to refer to the powder used for spraying and the primary particles that constitute the secondary particles. 50 "50% volume average particle size" refers to the average particle size of the cumulative 50% of the particle size distribution on a volume basis, as measured by a particle size distribution measuring device based on laser scattering / diffraction. In this specification, "average particle size (D)" is sometimes used instead of "average particle size". 50 ")" is also called "D" v50 ".
[0061] <Methods for measuring the angle of rest>
[0062] In this specification, the term "stationary angle" refers to the base angle calculated based on the diameter and height of the conical deposit formed when spray-coating powder is dropped from a funnel of a certain height onto a horizontal substrate. The stationary angle can be measured according to JISR 9301-2-2:1999 "Methods for determination of physical properties of alumina powder - 2: Stationary angle".
[0063] <Methods for determining bulk density>
[0064] In this specification, the term "bulk density" related to spray plating powder means: the density (specific gravity) calculated based on the mass of the spray plating powder when it is filled to a specified capacity container by naturally filling it with spray plating powder that flows naturally from a 2.5 mm diameter orifice. Bulk density can be determined according to JIS Z2504:2012 "Metal powders - Method for determination of apparent density".
[0065] <Methods for determining particle strength (compressive strength)>
[0066] In this specification, the "particle strength" related to the powder used for spraying is measured using a compression testing machine with electromagnetic force loading. Specifically, the test specimen is fixed between a pressure head and a pressure plate, and a load force is applied using electromagnetic force at a certain increasing ratio. Compression is performed at a constant load rate, and the amount of deformation of the test specimen is measured. The deformation characteristics of the measured specimen are processed using a dedicated program to calculate the strength value.
[0067] <Composition of Powder for Spraying>
[0068] The spray-coating powder disclosed herein is a spray-coating powder used in the production of a spray-coated film using a spray-coating method. As described above, this spray-coating powder is composed of ceramic particles. The proportion of ceramic particles in the spray-coating powder is preferably 95% by mass or more, more preferably 99% by mass or more, and even more preferably 99.9% by mass or more, for example, it can be set to 99.99% by mass or more. The type of ceramic can be appropriately selected according to the composition of the spray-coated film to be produced. Examples of ceramics include oxide ceramics formed from oxides, carbides, borides, nitrides, apatite, and other non-oxide ceramics.
[0069] As an oxide ceramic, there are no particular limitations; various metal oxides can be used. Metallic or non-metallic elements constituting this oxide ceramic may include, for example, one or more selected from the following: half-metallic elements such as boron (B), silicon (Si), germanium (Ge), antimony (Sb), and bismuth (Bi); typical elements such as magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), zinc (Zn), aluminum (Al), gallium (Ga), indium (In), tin (Sn), and lead (Pb); transition metal elements such as scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), silver (Ag), and gold (Au); and lanthanide elements such as lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Er), and lutetium (Lu). Preferably, one or more elements are selected from Mg, Y, Ti, Zr, Cr, Mn, Fe, Zn, Al, and Er.
[0070] Examples of oxide ceramics include alumina, zirconium oxide, yttrium oxide, chromium oxide, titanium oxide, cobalt oxide, magnesium oxide, silicon dioxide, calcium oxide, cerium oxide, ferrite, spinel, zircon, nickel oxide, silver oxide, copper oxide, zinc oxide, gallium oxide, strontium oxide, scandium oxide, samarium oxide, bismuth oxide, lanthanum oxide, lutetium oxide, hafnium oxide, vanadium oxide, niobium oxide, tungsten oxide, manganese oxide, tantalum oxide, terbium oxide, europium oxide, neodymium oxide, tin oxide, antimony oxide, antimony-containing tin oxide, indium oxide, tin-containing indium oxide, zirconium aluminate, zirconium silicate, hafnium aluminate, hafnium silicate, titanium silicate, lanthanum silicate, lanthanum aluminate, yttrium silicate, titanium silicate, tantalum silicate, etc.
[0071] Examples of non-oxide ceramics include carbide ceramics such as tungsten carbide, chromium carbide, vanadium carbide, niobium carbide, molybdenum carbide, tantalum carbide, titanium carbide, zirconium carbide, hafnium carbide, silicon carbide, and boron carbide; boride ceramics such as molybdenum boride, chromium boride, hafnium boride, zirconium boride, tantalum boride, and titanium boride; nitride ceramics such as titanium nitride, silicon nitride, and aluminum nitride; composites such as forsterite, steatite, cordierite, mullite, barium titanate, lead titanate, lead zirconate titanate, Mn-Zn ferrite, Ni-Zn ferrite, and silane; and phosphate compounds such as hydroxyapatite and calcium phosphate.
[0072] In the ceramics described above, any element can be doped or substituted. Furthermore, these ceramics can contain one or more of these elements individually or in combination. For example, when containing two or more ceramic elements, they can partially or completely form a composite. Examples of such composite ceramics include yttrium-stabilized zirconium oxide, partially stabilized zirconium oxide, gadolinium-doped cerium oxide, lanthanum-doped lead zirconate titanate, the aforementioned silane, and the aforementioned composite oxides.
[0073] The spray-coating powder disclosed herein is characterized in that, compared to before spray-coating, the average particle size (D) of the spray-coating powder is [value missing] after atmospheric pressure plasma spraying in water under the following conditions. 50 The value of ) should be reduced by at least 25%.
[0074] The conditions are as follows:
[0075] Plasma working gas:
[0076] Argon (Ar): 50 psi; and
[0077] Helium (He): 50 psi
[0078] Plasma output: 36kW
[0079] Powder feed rate for spraying: 20g / min
[0080] Spraying distance: 400mm
[0081] The degree of thermal shrinkage of the powder used for spraying can be determined, for example, by utilizing the average particle size (D) of the powder used for spraying resulting from atmospheric pressure plasma spraying under the conditions described above. 50 The reduction rate (%) (hereinafter also referred to as "D") 50 The reduction rate (%) is used for evaluation. It should be noted that the plasma output value may contain a certain amount of error. The plasma output value is typically the arithmetic mean.
[0082] The average particle size (D) of the powder used for spraying before atmospheric pressure plasma spraying is defined as follows:50 Let D1 be the average particle size (D) of the spraying powder recovered from the water after spraying. 50 When set to D2, the D of the powder used for spraying is... 50 The reduction rate (%) can be calculated using the following formula (1).
[0083] D 50 Reduction rate (%) = (D1-D2) / D1×100 (1)
[0084] D of powder for spraying 50 The reduction rate (%) is 25% or more, preferably 30% or more, and more preferably 35% or more, as described above. 50 The higher the reduction rate (%), the denser and smoother the sprayed film can be produced.
[0085] Alternatively, the D of the powder used for spraying before and after atmospheric pressure plasma spraying (APS) can also be analyzed. 10 Or D 90 The degree of thermal shrinkage of the powder used for spraying can be compared and evaluated. For example, it can also be measured by D. 10 Reduction rate (%) or D 90 The reduction rate (%) is the indicator used in this evaluation. It should be noted that D... 10 This refers to the cumulative 10% of the particle size from the smallest particle size side in the particle size distribution of a volume reference, as measured using a particle size distribution measurement device based on laser scattering / diffraction. (D) 90 It refers to the particle size that accounts for 90% of the cumulative value from the smallest particle size side in the particle size distribution of a volume reference, as measured by a particle size distribution measuring device based on laser scattering / diffraction.
[0086] D of powder for spraying 10 The reduction rate (%) can be calculated using the following formula (2).
[0087] (D before APS above) 10 -D after the above APS 10 ) / D before the above APS 10 ×100 (2)
[0088] The reduction rate (%) of D10 of the powder used for spraying is preferably 15% or more, more preferably 20% or more, and even more preferably 25% or more. 10 The higher the reduction rate (%), the denser and smoother the sprayed film can be produced.
[0089] D of powder for spraying 90 The reduction rate (%) can be calculated using the following formula (3).
[0090] (D before APS above) 90 -D after the above APS 90) / D before the above APS 90 ×100 (3)
[0091] D of powder for spraying 90 The reduction rate (%) is preferably 35% or more, more preferably 40% or more, and even more preferably 45% or more. 90 The greater the reduction rate (%), the finer the powder used for spraying can be, which in turn allows for the production of a denser and smoother sprayed film.
[0092] The stationary angle of the spray-coating powder disclosed herein can be 40 degrees or less. The stationary angle has long been a widely used indicator to represent the flowability of powder. The stationary angle of the spray-coating powder can serve as an indicator of the flowability of the powder within the supply device, during transport from the supply device to the spray-coating device, etc. Therefore, the smaller the stationary angle is specified, the more flowable the spray-coating powder can be, and consequently, the more efficiently a homogeneous spray-coated film can be produced. The stationary angle of the spray-coating powder is preferably 39 degrees or less, more preferably 38 degrees or less, and even more preferably 37 degrees or less. There is no particular limitation on the lower limit of the stationary angle, but if the stationary angle is too small, the spray-coating powder may become prone to scattering, or the control of the powder supply may become difficult. From this viewpoint, it is preferable to set the stationary angle of the spray-coating powder to 20 degrees or more. It should be noted that the stationary angle here refers to the stationary angle before the aforementioned APS.
[0093] The bulk density of the spray coating powder disclosed herein can be 3.0 g / cm³. 3 The following describes the bulk density, which can be used as an indicator of the ease with which the powder for spraying can undergo thermal shrinkage during spraying. Therefore, the lower the bulk density, the easier it is to achieve thermal shrinkage of the powder for spraying, and consequently, a denser sprayed film can be produced. For example, the bulk density of the powder for spraying is 2.0 g / cm³. 3 The preferred value is 1.5 g / cm³. 3 The preferred value is 1.2 g / cm³. 3 The following is a further preferred value of 1.0 g / cm³. 3 The following should be noted: If the bulk density is too low, the productivity of the spray-coated film may sometimes decrease. From this perspective, the bulk density of the powder used for spray coating is set to 0.5 g / cm³. 3 The above is recommended. It should be noted that the bulk density here refers to the bulk density before the APS mentioned above.
[0094] The particle strength (compressive strength) of the spray coating powder disclosed herein can be 0.7 kgf / mm². 2 The above. The preferred particle strength is 0.9 kgf / mm². 2 The above, more preferably 1.0 kgf / mm 2The above explains why, by setting the particle strength (compressive strength) within this range, the scattering and disintegration of the powder during spraying and feeding into the spraying equipment can be suppressed, thereby enabling the production of a homogeneous sprayed film with better productivity. On the other hand, if the particle strength is too high, it can sometimes be difficult to fully melt the powder. From this perspective, a particle strength of 500 kgf / mm² is suitable for spraying powder. 2 The following is appropriate, preferably 400 kgf / mm 2 Below, 200 kgf / mm is more preferred. 2 The following should be noted: the particle strength here refers to the particle strength before the APS mentioned above.
[0095] The average particle size (D) of the powder used for spraying is disclosed herein. 50 The average particle size can be greater than 10 μm. 50 The average particle size (D) is preferably 14 μm or more, more preferably 18 μm or more, and even more preferably 22 μm or more. 50 Setting the particle size to this range allows the flowability of the powder for spraying to be suitable for the powder supply, thereby enabling the production of a homogeneous sprayed film with better productivity. On the other hand, the average particle size (D...) 50 For example, it can be set to 55 μm or less, preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 35 μm or less. This is achieved by adjusting the average particle size (D...) 50 Setting the average particle size (D) to this range allows the powder to be fully melted during spraying. In one example, it is particularly preferable to set the average particle size (D) within this range. 50 The average particle size (D) is set to 20μm to 30μm. This allows for optimal flowability of the powder used in spraying and produces a dense and smooth sprayed film. It should be noted that the average particle size (D) here refers to... 50 The average particle size (D) before APS is mentioned above. 50 ).
[0096] Furthermore, the particle size distribution of the powder for spray coating disclosed herein can be appropriately set according to the type and conditions of the equipment used in the spray coating process for producing the spray-coated film. For example, the D of the powder for spray coating... 90 The setting can be below 60μm (e.g., below 50μm). The D of the powder used for spraying... 10 It can be set to below 20μm. It should be noted that D here... 90 and D 10 D before the above APS 90 and D 10 .
[0097] When the ceramic particles constituting the spraying powder disclosed herein are secondary particles, the average particle size D of the primary ceramic particles constituting the secondary particles is... 50 It can be below 10 μm. Average particle size D50 Preferably, it is 9 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less. This is achieved by adjusting the average particle size D... 50 When the powder is set to this range, heating based on the heat source becomes easier to reach the center of the primary particles during spraying. Therefore, it is possible to suppress the mixing of spraying powder, including unmelted portions due to insufficient heating, into the sprayed film, thereby enabling the production of a denser sprayed film. On the other hand, the average particle size D... 50 The average particle size D can be set to 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more. 50 Setting it to this range can suppress defects in the sprayed film that are thought to be caused by overheating, and can produce a denser sprayed film.
[0098] From the perspective of thermal shrinkage as described above, the spray coating powder disclosed herein is preferably a granulated sintered powder. This spray coating powder is, for example, a spray coating powder composed of granulated sintered particles, which are secondary particles formed by mixing and granulating raw material particles (primary particles) of ceramic particles, followed by sintering, and are formed by three-dimensionally bonding the primary particles with gaps between them. In other words, the ceramic particles constituting this spray coating powder can be granulated sintered particles of primary particles formed from ceramic. Hereinafter, an example of a suitable granulation and sintering method for producing such granulated sintered particles will be described, but it is not intended to limit the scope to this method.
[0099] <Method for manufacturing powder for spraying>
[0100] Granulation and sintering is a method in which raw material particles (primary particles) are granulated into secondary particles and then sintered to firmly bond the particles together. In this granulation and sintering method, granulation can be carried out using methods such as dry granulation or wet granulation. Examples of granulation methods include rotary granulation, fluidized bed granulation, stirred granulation, crushing granulation, melt granulation, spray granulation, and microemulsion granulation. Among these, spray granulation is a suitable granulation method.
[0101] Based on the spray granulation method, spray plating powder can be manufactured, for example, by the following steps: First, raw material particles with a desired composition are prepared, and their surfaces are stabilized using a protective agent or the like as needed. Then, the stabilized raw material particles, along with spacer particles formed from organic materials or the like as needed, and binders and various additives (e.g., dispersants) as arbitrary components, are dispersed together in a suitable solvent to prepare a spray liquid. The dispersion of the raw material particles in the solvent can be carried out, for example, using a homogenizer, a wing mixer, or a disperser. Then, the spray liquid is sprayed using an ultrasonic sprayer or the like to form droplets. These droplets are placed in an airflow and passed through a spray drying device (spray dryer), thereby forming granulated particles. The resulting granulated particles are introduced into a prescribed sintering furnace for sintering, thereby sintering the raw material particles. In this way, a spray plating powder composed of granulated sintered particles in the form of secondary particles formed by the intermittent bonding of primary particles can be obtained. It should be noted that the primary particles here can have almost the same size and shape as the raw material particles, or the raw material particles can grow / bond through sintering.
[0102] To impart the required thermal shrinkage properties to the granulated sintered particles (powder for spraying) thus manufactured, it is preferable to use isolating particles in the preparation of the aforementioned spray liquid. In this way, in the aforementioned manufacturing process, the raw material particles, isolating particles, and binder are uniformly mixed in the dry droplet state. The raw material particles and isolating particles are bonded together by the binder to form mixed particles. This mixed particle is then sintered, causing the isolating particles and binder to disappear (burn off), and the raw material particles are sintered. This forms secondary particles with a gapped bond between the primary particles. It should be noted that during sintering, depending on their composition and size, a portion of the raw material particles becomes liquid, which facilitates bonding with other particles. Therefore, the average particle size of the primary particles may sometimes be larger than that of the initial raw material particles. Furthermore, during the period from drying to sintering, due to the disappearance of components other than the raw material particles and the sintering of the raw material particles caused by sintering, the average particle size of the resulting secondary particles is significantly reduced compared to the droplet size. The average particle size of these secondary particles and primary particles, as well as the size and proportion of the gaps formed between primary particles, can be appropriately designed according to the desired morphology of the secondary particles.
[0103] When the isolating particles disappear from the mixed particles during sintering of the granulated particles, pores are generated in the portion of the mixed particles where the isolating particles were present. Therefore, by using isolating particles, the porosity of the granulated sintered particles can be increased. By increasing the porosity of the granulated sintered particles, the degree of thermal shrinkage of the granulated sintered particles (i.e., powder for spraying) based on spraying can be increased. The porosity of the granulated sintered particles can be appropriately adjusted by the amount of isolating particles added, particle size, shape, etc. For example, the mixing ratio of raw material particles to isolating particles (volume of raw material particles: volume of isolating particles) is preferably 80:20 to 10:90. The higher the mixing ratio (volume ratio) of isolating particles, the higher the porosity of the granulated sintered particles can be, and thus, the more dense and smooth the sprayed film can be produced. From this viewpoint, when the total volume of raw material particles and the volume of isolating particles is set to 100% by volume, the volume ratio of isolating particles is more preferably 30% by volume or more, and even more preferably 40% by volume or more. On the other hand, in order to improve the physical stability and processability of the sprayed powder and produce a more homogeneous sprayed film with better productivity, it is appropriate for the volume ratio of the isolation particles to be 80% by mass or less, and preferably 70% by volume or less.
[0104] The particle size of the isolation particles is, for example, 0.1 μm to 10 μm, preferably 1 μm to 5 μm. The isolation particles can be made from so-called pore-forming materials used for producing such granulated sintered particles (e.g., acrylic resin particles, epoxy resin particles, polyimide resin particles, polyolefin particles, etc.). Furthermore, the shape of the isolation particles is not particularly limited; for example, they can be spherical or substantially spherical, plate-like, fibrous, etc.
[0105] Furthermore, in the aforementioned manufacturing process, the concentration of the raw material particles in the adjusted spray liquid is preferably 10% to 50% by mass. Additionally, the amount of binder added is preferably adjusted to a ratio of 0.05% to 10% by mass (e.g., 1% to 5% by mass) relative to the mass of the raw material particles. Examples of added binders include carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), and polyvinylpyrrolidone (PVP).
[0106] Furthermore, in the aforementioned manufacturing process, firing can be carried out in the atmosphere, in a vacuum, or in an inert gas atmosphere. To remove the aforementioned separating particles and binder, firing is preferably carried out in an oxygen-containing atmosphere. The firing temperature can be set, for example, to 600°C or higher and 1600°C or lower. It should be noted that after firing, the manufactured secondary particles can be crushed and / or graded as needed.
[0107] When SEM observation was performed on the surface of the spraying powder composed of granulated sintered particles manufactured as described above, it was found that the granulated sintered particles have a ceramic matrix portion. Figure 3 The white part), and the opening ( Figure 3 (The black portion). These openings are independent, separate openings formed by burning away the isolation particles from the mixture of raw material particles and isolation particles formed in the aforementioned manufacturing process during firing. As described in the embodiments below, the matrix portion and the independent opening portion in the granulated sintered particles can be separated by using commercially available image analysis software.
[0108] The aforementioned independent openings can be approximately circular in shape. "Approximately circular in shape" means that the ratio (Dmax / Dmin) of the maximum diameter Dmax to the minimum diameter Dmin of the independent opening is between 1 and 1.8. This ratio (Dmax / Dmin) can be determined by observing the surface of the sprayed powder using SEM and performing image analysis on the obtained surface SEM image. For example, randomly selecting 5 or more (e.g., 10 or more) ceramic particles from the surface SEM image, the ratio (Dmax / Dmin) is calculated for the independent openings within an imaginary circle with a diameter equal to half the particle's diameter, starting from the center of each particle. Furthermore, in the calculation, particles smaller than 1 μm during binarization are considered. 2 The exclusion of minute regions is ideal. This allows us to obtain an arithmetic mean that more closely approximates the true state. The arithmetic mean of the values calculated here is then used to evaluate the shape of individual openings.
[0109] The aforementioned individual openings can each have approximately the same diameter. "Approximately the same diameter" means, for example, that the average diameter of the individual openings relative to the Dmax and Dmin used in the above-mentioned ratio (Dmax / Dmin) measurement is within 20% (preferably within 10%). It should be noted that the diameter of the individual opening can be -20% to +20% of the length relative to the size of the separating particles used in the above-mentioned manufacturing process.
[0110] The aforementioned independent openings can exist on average in one granulated sintered particle with more than 20 openings. The more independent openings exist on the surface of the granulated sintered particle, the greater the thermal shrinkage of the powder for spraying becomes, and thus, a denser and smoother sprayed film can be produced. In one granulated sintered particle, the number of independent openings on average is preferably more than 30, more preferably more than 40, and even more preferably more than 50. On the other hand, considering the flowability and particle strength of the powder for spraying, the number of independent openings in one granulated sintered particle can be set to less than 200 (for example, less than 150 or less, or less than 100) on average. It should be noted that the number of independent openings can be counted from 5 or more (for example, more than 10) ceramic particles randomly extracted from the surface SEM image, and their arithmetic mean can be obtained.
[0111] Alternatively, in the powder for spraying manufactured using the above method, the porosity of the surface of the granulated sintered particles can be 20% or more, calculated on an average basis. To achieve this porosity, when observing multiple surface SEM images of granulated sintered particles (e.g., 5 to 10 images), the ratio of the total area of the openings (independent openings) to the area (projected area) of any number of particles (e.g., 1 to 5 per image) used as the analysis object in each image is measured, and the average value is taken. It should be noted that only approximately half of the particle can be observed in the surface SEM image, but by setting the area of this half-face and the pore area to twice the original value, the overall surface area and pore area of the particle can be easily obtained.
[0112] Porosity is one of the indicators for evaluating the porosity of granulated sintered particles, preferably 25% or more, more preferably 30% or more. Higher porosity increases the thermal shrinkage of the powder used for spraying, resulting in a denser and smoother sprayed film. On the other hand, considering the physical stability and processability of the sprayed powder, the porosity is, for example, 70% or less, preferably 60% or less, more preferably 50% or less. It should be noted that the specific method for measuring porosity is as described in the examples below.
[0113] The following is for reference Figure 1 , 2 The mechanism by which the thermal shrinkage of the spray-plating powder disclosed herein is improved compared to conventional methods will be explained. However, it is not intended that the mechanism for achieving the effect of the spray-plating powder disclosed herein be limited to the following. Figure 1 As shown, when ceramic particles 11 constituting the spraying powder disclosed herein are sprayed, the ceramic particles 11 become molten flying particles 12 due to the heat energy during spraying. When the flying particles 12 reach the substrate S, a sprayed film L1 is formed. If the ceramic particles 11 melt, the molten ceramic enters the gaps P1 (open and closed pores). In other words, the volume of the gaps decreases. Therefore, the flying particles 12 during spraying shrink compared to before spraying. Thus, the flying particles 12 that shrink due to spraying form the sprayed film L1, thereby increasing the density of the sprayed film L1 and further improving the smoothness of the surface of the sprayed film.
[0114] When comparing the spraying powder disclosed herein with the spraying powder in a previous example, Figure 2The conventional ceramic particles 21 shown also contain gaps P2. However, the volume of the gaps in ceramic particles 21 is smaller than that in ceramic particles 11. Therefore, it can be considered that the degree of thermal shrinkage of ceramic particles 21 when they become flying particles 22 is less than that of ceramic particles 11. In addition, compared with ceramic particles 11, ceramic particles 21 have a higher internal density, and even if the particle surface melts due to spraying, sometimes the interior of the particle will reach the substrate S (unmelted particles 23) while remaining unmelted. Therefore, it is considered that the density and surface smoothness of the sprayed film L1 made by spraying ceramic particles 11 are improved compared with the density and smoothness of the sprayed film L2 made by spraying ceramic particles 21.
[0115] The spraying powder disclosed herein can be used to create sprayed films on various substrates by employing various spraying methods. The spraying powder disclosed herein is particularly preferred for creating sprayed films using atmospheric plasma spraying (APS), low-pressure plasma spraying (LPS), high-pressure plasma spraying, and other plasma spraying methods. It should be noted that this spraying powder is also suitable for high-speed flame spraying methods such as high-velocity oxygen flame (HVOF) spraying, warm spraying, and high-velocity air flame (HVAF) spraying. It should be noted that the spraying powder can be supplied to the spraying apparatus in powder form or in the form of a slurry dispersed in a suitable dispersion medium.
[0116] There are no particular restrictions on the types of substrates used to make the sprayed coating. Examples of substrates include aluminum, aluminum alloys, iron, steel, copper, copper alloys, nickel, nickel alloys, gold, silver, bismuth, manganese, zinc, and zinc alloys. Ideal examples include: steels such as those used as corrosion-resistant structural steels and various SUS materials (which can be called stainless steel), aluminum alloys such as the 1000 series to 7000 series aluminum alloys used as lightweight structural materials, and substrates formed from Ni-based, Co-based, and Fe-based corrosion-resistant alloys such as Hastelloy alloys, Inco nickel alloys, Stellite alloys, and Invar alloys.
[0117] Example
[0118] The following describes embodiments related to the present invention, but it is not intended to limit the present invention to the contents shown in the following embodiments.
[0119] <Manufacturing Example>
[0120] [Sample manufacturing]
[0121] (Sample 1)
[0122] As a raw material powder, the average particle size D 50 Yttrium oxide powder (primary particles) with a diameter of 0.9 μm and an average particle size D 50 Yttrium oxide powder (primary particles) with a particle size of 3.0 μm was mixed to prepare a mixed powder. As separator particles, acrylic resin separator particles (hereinafter also referred to as "acrylic particles") with a particle size (particle diameter) of approximately 3 μm were prepared (MX-300, manufactured by Soken Chemical Co., Ltd.). The above mixed powder was mixed to a concentration of 70 vol% and acrylic particles to a concentration of 30 vol%, and dispersed in an aqueous solution containing 2 wt% binder to prepare a spray liquid. In the spray liquid, the content of yttrium oxide particles was 90.7 wt% and the content of acrylic particles was 9.3 wt%. The spray liquid was sprayed in an airflow using a spray granulator to dry it, thereby producing granulated particles. The obtained granulated particles were sintered at 1600°C to sinter the primary particles, and then crushed and graded to manufacture a spray-coating powder composed of granulated sintered particles (secondary particles). This spray-coating powder is Sample 1 of this manufacturing example. The average particle size D of Sample 1 is... 50 It is 27μm.
[0123] (Sample 2)
[0124] The above-mentioned formulation, consisting of 40% by volume of mixed powder and 60% by volume of acrylic particles, was used. In the spray solution, the content of yttrium oxide particles was 73.5% by weight, and the content of acrylic particles was 26.5% by weight. Except for this, the same materials and processes as for Sample 1 were used to manufacture the spraying powder for Sample 2. The average particle size D of Sample 2 was... 50 It is 27μm.
[0125] (Sample 3)
[0126] As a raw material powder, the average particle size D is used 50 Yttrium oxide powder (primary particles) with a particle size of 2.4 μm was used. Acrylic particles were not used. The powder for spraying of sample 3 was manufactured using the same materials and processes as sample 1. The average particle size D of sample 3 is... 50 It is 27μm.
[0127] (Sample 4)
[0128] As Sample 4, molten yttrium oxide powder was prepared. First, a raw material powder was prepared in a manner consistent with obtaining the target yttrium oxide (Y₂O₃). This raw material powder was heated to melt and then cooled to prepare a solidified product (ingot). The solidified product was then mechanically pulverized and graded as needed, thereby obtaining the molten yttrium oxide powder of Sample 4. The average particle size D of Sample 4 is... 50 It is 29μm.
[0129] [Determination of Particle Size Distribution]
[0130] For the spraying powders of samples 1–4, the particle size distribution on a volume basis was determined using a laser diffraction / scattering particle size analyzer (Malvern Panalytical, Mastersizer 3000). The corresponding column in Table 1 shows D. v10 D v50 and D v90 The value of .
[0131] [Angle of rest]
[0132] For the spraying powders of samples 1 to 4, the stationary angle was measured according to JIS R9301-2-2:1999. The stationary angle was obtained by feeding each spraying powder to an ABD powder property measuring instrument (manufactured by Riko Tsutsui Instruments Co., Ltd., ABD-72 type). The corresponding columns in Table 1 show the measured stationary angle values.
[0133] [Determination of bulk density]
[0134] For the spraying powders of samples 1–4, the bulk density (g / cm³) was determined according to JIS Z2504:2012. 3 Bulk density (g / cm³) 3 The values are obtained using a JIS bulk density tester (manufactured by Tsutsui Rikko Chemical Equipment Co., Ltd.) for supplying various spraying powders to metal powders. The corresponding columns in Table 1 show the measured bulk density (g / cm³). 3 The value of ).
[0135] [SEM Observation]
[0136] For the spraying powders of samples 1-4, top-view and cross-sectional images were obtained using a benchtop SEM (Phenom-World, Phenom ProX). The magnification was 5000x. For reference, Figures 3-8 The surface SEM images and cross-sectional SEM images of samples 1-3 are shown. Figures 3-8 The scale bars in the image represent 10 μm.
[0137] Porosity of particle surface
[0138] For the powder used in spraying samples 1-4, the ratio of the area containing pores to the total surface area of the particles was measured (porosity of the particle surface (%)). For the surface SEM images of each sample obtained in the [SEM observation] section above, image analysis software (NIPPON ROPER KK, Image-Pro Plus) was used, and only the particle portion of the surface SEM image was specified for binarization. Specifically, a contrast threshold was determined, and the white portion was set as the matrix (yttrium oxide) portion, and the black portion as the pores. Then, the ratio of the area containing pores was calculated when the area (projected area) of the object being analyzed was set to 100%. This measurement was performed on 10 randomly selected ceramic particles. The arithmetic mean obtained was then used as the porosity (%) of the particle surface of each sprayed material. The corresponding columns in Table 1 show the measured values of the porosity (%) of the particle surface.
[0139] [Table 1]
[0140] Table 1
[0141]
[0142] As shown in the results of this manufacturing example Figures 3-8 As shown in Table 1, in the spray-coating powders (samples 1 and 2) obtained by granulation and sintering using a spray liquid containing yttrium oxide particles and a specified amount of isolation particles (acrylic particles), open and closed pores caused by the disappearance of isolation particles due to sintering were observed. Furthermore, in the spray-coating powders of samples 1 and 2, the porosity of the particle surface was 20% or more, and this porosity increased depending on the amount of isolation particles. On the other hand, regardless of whether isolation particles were used, the particle size distribution of the spray-coating powders of samples 1 to 3, which consisted of granulated and sintered particles, was the same. In addition, the stationary angle of the spray-coating powders of samples 1 to 4 was 40 degrees or less, confirming that they possessed flowability suitable for spray coating. Furthermore, it was confirmed that by using isolation particles to produce granulated and sintered particles, the bulk density of the spray-coating powder decreased.
[0143] <Making Flying Particles>
[0144] The powder for spraying of samples 1 to 4 manufactured in the above manufacturing example was subjected to atmospheric pressure plasma spraying (APS) in water under the following spraying conditions to produce flying particles for each sample.
[0145] [Spraying conditions]
[0146] Spray plating machine: SG-100 (manufactured by Praxair)
[0147] Powder feeder: Model 1264 (manufactured by Praxair)
[0148] Plasma working gas:
[0149] Argon (Ar) gas (50 psi (0.34 MPa)); and
[0150] Helium (He) gas (50 psi (0.34 MPa))
[0151] Plasma output: 36kW
[0152] Plasma generation voltage: 40V
[0153] Plasma generation current: 900A
[0154] Powder feed rate for spraying: 20g / min
[0155] Spraying distance: 400mm
[0156] In the production of flying particles, firstly, in the aforementioned spray coating machine, Ar (primary gas) and He (secondary gas) are supplied as plasma working gases at atmospheric pressure. A voltage is applied between the cathode and anode, thereby generating plasma. The plasma generation conditions during spray coating are as described above. It should be noted that the plasma generation current is set to 900A, and the plasma generation voltage varies within the range of 38-42V, thus the plasma output can vary within the range of 34-38kW. In this plasma process, the aforementioned powder supply machine supplies the spray coating powder for each sample, which is then sprayed into cold water. The plasma irradiation angle relative to the water surface is 90 degrees. It should be noted that the aforementioned "spray coating distance" related to the production of flying particles refers to the distance from the tip of the spray coating gun to the water surface.
[0157] As described above, water is recovered after spraying the powder by atmospheric pressure plasma sputtering. The sprayed powder (ceramic particles) contained in the recovered water is dried to produce flying particles for each sample. For reference, Figures 9-11 SEM images of each sample are shown (magnification 1000x). Figures 9-11 The scale bar indicates 80μm.
[0158] [Determination of particle size reduction rate]
[0159] Similar to the determination of the particle size distribution of the spraying powder in the above manufacturing examples, the particle size distribution of the flying particles in each example was measured based on a volumetric standard. The particle size distribution of the flying particles was then determined using the D... v10 D v50 and D v90 And the D of the powder used for spraying before APS mentioned above v10 D v50 and D v90The reduction rate (%) of each particle size of the spraying powder for each sample based on APS was calculated. Specifically, based on the above equations (1) to (3), the D before and after APS was calculated. v10 D v50 and D v90 The reduction rate (%), as D v10% Reduction rate (%), D v50% Reduction rate (%) and D v90% Reduction rate (%). The corresponding column in Table 2 shows the D after APS. v10 D v50 and D v90 The values of the reduction rate (%) for each particle size.
[0160] [Table 2]
[0161] Table 2
[0162]
[0163] As shown in Table 2, it can be confirmed that in any sample, the D of ceramic particles before and after APS... v10 D v50 and D v90 All decreased (D of sample 4) v10 (Except for). A comparison was made between spraying powders (samples 1 and 2) composed of granulated sintered particles manufactured using isolation particles and spraying powders (samples 3 and 4) of examples not using isolation particles, and it was confirmed that the particle size reduction rate (%) of samples 1 and 2 was greater than that of samples 3 and 4.
[0164] <Production of Spray Coating>
[0165] Using the plating powder of samples 1-4 manufactured in the above-described manufacturing example, a plating film was made using APS. In this example, the substrate was a roughened surface of a sheet (70mm × 50mm × 2.3mm) made of aluminum alloy (Al6061) that had been sandblasted with brown alumina abrasive material (A#40). The apparatus, plasma generation conditions, and supply speed of the plating powder used in this example were the same as those in the "Preparation of Flying Particles" described above. In this example, the plating powder for each sample was supplied to the plasma generated in the above-described plating machine, and the plating gun was moved at a speed of 400mm / s while the plasma irradiation angle relative to the substrate was 90 degrees to create plating films for samples 1-4. It should be noted that the plating distance was set to 90mm-130mm. The "plating distance" mentioned above in relation to the preparation of the plating film refers to the distance from the tip of the plating gun to the substrate. For reference, Figures 12-14 The cross-sectional SEM images of the sprayed films of samples 1-3 are shown (1000x magnification). Figures 12-14The scale bar in the image represents 80 μm.
[0166] [Film formation rate]
[0167] Using the spraying powders from samples 1 to 4, the film formation rate (μm / pass) in the fabrication of the above-mentioned sprayed films was calculated. This film formation rate (μm / pass) is the thickness (μm) of the sprayed film produced by the spraying apparatus (spraying gun) performing one spraying operation (1 pass) along the operating direction of the spraying apparatus. Representative film formation rates (μm / pass) for each sample are shown in the corresponding columns of Table 3. It should be noted that the values recorded in the "Spraying Distance" column of Table 3 are the spraying distances at which the film formation rate, the following density, and the following surface roughness measurements were obtained.
[0168] [Denseness]
[0169] The compactness of the sprayed films of samples 1-4, formed as described above, was evaluated by measuring the porosity (%) of the sprayed film. The porosity was determined by image analysis of SEM images of cross-sections approximately perpendicular to the substrate. First, the sprayed film, along with the substrate, was cut perpendicularly to the substrate surface to obtain an arbitrary cross-section in the thickness direction. The cross-sectional SEM image of the sprayed film at this cross-section was analyzed using image analysis software (NIPPON ROPER KK, Image-Pro Plus), thereby separating the pore portion and the solid phase into binary values, and calculating the porosity (%) defined as the proportion of the pore area to the total cross-sectional area. Representative porosities (%) of each sample are shown in the corresponding columns of Table 3.
[0170] [Surface Roughness Measurement]
[0171] For the spray-coated films of samples 1–4, the surface roughness (arithmetic mean roughness) Ra was measured according to JIS B0601:2013. The surface roughness Ra was obtained by measuring the surface roughness of any 5 points on each spray-coated film using a surface roughness measuring machine “SV-3000S CNC” (manufactured by Mitutoyo Co., Ltd.), and using their arithmetic mean as the surface roughness Ra value. Representative surface roughness Ra (μm) for each sample is shown in the corresponding column of Table 3. Additionally, for reference, Figure 15 The surface roughness Ra (μm) of the sprayed film produced by spraying the powder for spraying of samples 1 to 3 at a spraying distance of 90 mm or 100 mm is shown. Figure 15 The vertical axis “Ra / μm” in the chart represents the surface roughness Ra (μm). Figure 15 The horizontal axis "Spraying distance / mm" in the chart represents the spraying distance (mm). Figure 15In the chart, in each region divided by each spraying distance, the left bar represents sample 1, the middle bar represents sample 2, and the right bar represents sample 3.
[0172] [Table 3]
[0173] Table 3
[0174]
[0175] As shown in Table 3, the film formation rate was the same for all samples when using the spraying powder, regardless of the powder preparation method. Furthermore, compared to the sprayed films prepared using the powder prepared with separator particles (samples 1 and 2), which were prepared using the powder prepared without separator particles (samples 3 and 4), the surface roughness Ra (μm) of the sprayed films of samples 1 and 2 was found to be smaller than that of the sprayed films of samples 3 and 4. Additionally, the porosity (%) of the sprayed film of sample 2 was smaller than that of the other samples, indicating that the use of separator particles helps to produce a sprayed film with a flatter and denser surface.
[0176] Based on the above results, it is evident that using the spraying powder (samples 1 and 2) allows for the supply of finer particles to the substrate and the fabrication of a sprayed film. The spraying powder (samples 1 and 2) is characterized by containing ceramic particles. When the spraying powder is subjected to atmospheric pressure plasma spraying in water under specified conditions, compared to before spraying, the average particle size (D50) of the spraying powder is reduced by at least 25%. Using this spraying powder allows for the fabrication of a smoother sprayed film. Furthermore, it is considered suitable for fabricating a denser sprayed film.
Claims
1. A powder for spray plating, characterized in that, Composed of ceramic particles, When comparing the powder for spraying with the powder before and after atmospheric pressure plasma spraying in water under the following conditions, the average particle size (D) of the powder for spraying, based on laser diffraction scattering, is as follows: 50 The value of ) should be reduced by at least 25%. The ceramic particles are granulated and sintered particles formed from the primary particles of the ceramic. The average ratio of the area of pores on the surface of the ceramic particles, as observed by SEM, to the total surface area is more than 20%. The bulk density of the powder used for spraying is 1.2 g / cm³. 3 the following, The conditions are as follows: Plasma working gas: Argon (Ar) gas: 50 psi; and Helium (He): 50 psi Plasma output: 36kW Powder feed rate for spraying: 20g / min Spraying distance: 400mm.
2. The powder for spraying according to claim 1, wherein the stationary angle is less than 40 degrees.
3. The powder for spraying according to claim 1, wherein it is composed of oxide ceramic particles.
4. The powder for spraying according to any one of claims 1 to 3, wherein, The ceramic particles are granulated and sintered particles formed from primary particles of the ceramic. When the surface of the ceramic particles is observed by SEM, the ratio of the maximum diameter Dmax to the minimum diameter Dmin of the openings on the surface, i.e., Dmax / Dmin, is 1~1.
8.
5. The powder for spraying according to any one of claims 1 to 3, wherein, The average particle size (D) of the primary particles based on laser diffraction scattering method 50 The size ranges from 0.5μm to 5μm.
6. The powder for spraying according to any one of claims 1 to 3, wherein the bulk density is 1.0 or less.
7. A method for producing a spray-coated film, wherein, A spray-coated film is prepared by spraying the powder for spraying according to any one of claims 1 to 6 onto the surface of a substrate.
Citation Information
Patent Citations
JP1971030799Y1
Manufacture of lens
JP1987062716A
Composite cermet powder and manufacturing method therefor
JP2003301201A
Ceramic shell thermal spray powders and methods of use thereof
US20030129320A1