Preparation method of aluminum-based conductive coating on surface of composite material

Through low-pressure cold spraying process and powder ratio optimization, an aluminum-based conductive coating with high density, high hardness, high bonding strength and good wear resistance was prepared, which solved the problem of low density, poor bonding performance and resistance of flame-spraying aluminum layer. The problems of poor wear performance and high resistivity reduce the impact of aircraft weight gain.

CN119040871AActive Publication Date: 2024-11-29WUHU STATE-OWNED FACTORY OF MACHINING

Patent Information

Application Number
CN202411031419.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-29
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The carbon fiber composite material has poor electrical conductivity, which causes the electrostatic charge to accumulate on the surface area of ​​the aircraft after lightning strike, resulting in deep layering or ablation. The existing flame-sprayed aluminum conductive layer has low density, high oxidation rate, poor binding performance, and high resistivity. Increasing the coating thickness causes the aircraft to gain weight.

Method used

The aluminum-based conductive coating is prepared by low-pressure cold spraying technology. By regulating the particle size and proportion of Al, Ni, and Al2O3 powders, combined with infrared temperature measurement and mechanical processing, it achieves high density, high hardness, high bonding strength and good wear resistance. aluminum-based conductive coating.

Benefits of technology

A lower thickness of conductive layer can meet the usage requirements, reduce the impact of the coating on aircraft flight, improve the density, hardness and wear resistance of the conductive layer, and reduce the resistivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040871A_ABST
    Figure CN119040871A_ABST
Patent Text Reader

Abstract

The invention relates to the field of composite material surface aluminum-based conductive coatings, in particular to a preparation method of a composite material surface aluminum-based conductive coating, which comprises the following specific steps: S1, preparing a powder raw material; s2, preparing a low-pressure cold spraying coating; s3, coating performance detection; the preparation of the low-pressure cold spraying aluminum-based conductive coating on the surface of the composite material is realized by regulating and controlling the particle size and proportion of Al, Ni and Al2O3 in the powder raw material and matched low-pressure cold spraying process parameters. The low-pressure cold spraying Al-Ni-Al2O3 conductive coating has the advantages of high density, high hardness, high bonding strength, good wear resistance, low resistivity and the like, so that the conductive layer with relatively low thickness can meet the use requirements, and the influence of coating weight increment on aircraft flight is reduced; the problems that a flame aluminum spraying layer on the surface of the composite material is low in density, poor in bonding performance, poor in wear resistance and high in resistivity are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum-based conductive coatings on the surface of composite materials, in particular to a method for preparing the aluminum-based conductive coatings on the surface of composite materials. Background Art

[0002] Carbon fiber reinforced polymer composites have excellent properties such as high strength, corrosion resistance, and fatigue resistance. In recent years, they have been used more and more widely in the field of aviation manufacturing. Compared with metal materials, carbon fiber composites have poor electrical conductivity. After being struck by lightning, the static charge that cannot be released will accumulate on the surface of the aircraft, causing deep stratification or severe ablation of composite components, affecting their use. The commonly used solution is to use flame spraying to prepare an aluminum conductive layer on the surface of aircraft composite materials. However, due to the limitations of the flame spraying process itself, the aluminum spray layer has problems such as low density, high oxidation rate, poor bonding performance, and high resistivity. In order to reduce the resistance of the conductive layer, it is necessary to increase the thickness of the aluminum spray layer (generally a coating with a thickness of 0.2 mm is required), which results in a large increase in the weight of the aircraft and reduces the economic efficiency of the aircraft flight.

[0003] Carbon fiber composite materials have poor electrical conductivity. After being struck by lightning, the static charge that cannot be released will accumulate on the surface of the aircraft, causing deep delamination or severe ablation of composite components, affecting their use. The flame-sprayed aluminum layer on the surface of commonly used composite materials has low density, high oxidation rate, poor bonding performance, and high resistivity. A thicker aluminum spray layer is required to meet the use requirements, resulting in a larger weight gain of the aircraft. It is necessary to propose a preparation method to solve the problems of low density, poor bonding performance, poor wear resistance, and high resistivity of the flame-sprayed aluminum layer. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a method for preparing an aluminum-based conductive coating on the surface of a composite material.

[0005] A method for preparing an aluminum-based conductive coating on the surface of a composite material, the specific steps of which are as follows:

[0006] S1. Preparation of powder raw materials: selecting powders according to requirements, and then fully mixing the powders, using a powder mixer, at a rotation speed of 5 rpm to 15 rpm, mixing the two powders for 30 min to 60 min, thereby obtaining the final powder raw materials for low-pressure cold spraying;

[0007] S2. Low-pressure cold spray coating preparation:

[0008] S21: Select carbon fiber composite material as the matrix and prepare metallographic, microhardness and resistance test specimens; select LY12 aluminum alloy as the matrix and prepare wear resistance test;

[0009] S22: Add a top iron as support on the back of the area to be sprayed on the carbon fiber composite material, perform sandblasting on the area to be sprayed, and after sandblasting, use compressed air to blow the surface of the sample;

[0010] S23: Within 4 hours after powder mixing and within 2 hours after sandblasting, a low-pressure cold spray process is used to prepare an aluminum-based conductive coating on the surface of the sample. During the process, an infrared thermometer is used to monitor the surface temperature of the part in real time, and the temperature is not higher than 90°C;

[0011] S24: Use mechanical processing to grind the coating surface of the bonding strength sample to a roughness of Ra0.8μm, then perform sandblasting on the surface coating of the bonding strength sample and the bonding surface of the mating part, and stack the mating parts 4-FM1000 film-bonding strength sample in sequence, and apply a pressure of 5kg to 6kg at both ends. Put them into an oven while maintaining the pressure, and finally cool them with the furnace;

[0012] S25: Remove the supporting top iron on the back of the carbon fiber composite material sample. For the metallographic and friction and wear sample 7 surface coating, use 600 mesh, 800 mesh, 1000 mesh, and 2000 mesh sandpaper to polish it in turn, and then use 3μm diamond polishing liquid and 0.02μm silicon oxide polishing liquid to polish the coating.

[0013] S3. Coating performance test:

[0014] S31. Visually inspect the surface of the low-pressure cold-sprayed aluminum-based conductive layer. The coating should be free of cracks, warping, peeling or shedding.

[0015] S32. Observe the microstructure of the low-pressure cold-sprayed aluminum-based conductive layer using a scanning electron microscope, and analyze the porosity of the coating with reference to relevant standards;

[0016] S33, using an automatic micro-Vickers hardness tester to measure the microhardness of the low-pressure cold-sprayed aluminum-based conductive layer;

[0017] S34. Evaluate the bonding strength of the low-pressure cold-sprayed aluminum-based conductive layer with reference to the relevant standards;

[0018] S35. By means of a friction and wear tester, the wear resistance of the low-pressure cold-sprayed aluminum-based conductive layer was tested by using a ball-on-disc wear tester and using Si3N4 ball 6 as a counter-wear member under a load of 10N and a linear speed of 125mm / s for 10min;

[0019] S36. With the help of BT3562A resistance measuring instrument, the resistance of the low-pressure cold-sprayed aluminum-based conductive layer was measured using a four-probe method.

[0020] The beneficial effects of the present invention are as follows: the present invention realizes the preparation of a low-pressure cold-sprayed aluminum-based conductive coating on the surface of a composite material by regulating the particle size and proportion of Al, Ni, and Al2O3 in powder raw materials, as well as the matching low-pressure cold spraying process parameters; the low-pressure cold-sprayed Al-Ni-Al2O3 conductive coating has the advantages of high density, high hardness, high bonding strength, good wear resistance, and low resistivity, so that a conductive layer of lower thickness can meet the use requirements, reducing the impact of coating weight gain on aircraft flight, and effectively solving the problems of low density, poor bonding performance, poor wear resistance, and high resistivity of the flame-sprayed aluminum layer on the surface of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0022] Figure 1 It is a schematic diagram of the structure of the wear-resistant specimen of the present invention;

[0023] Figure 2 It is a schematic diagram of the bonding strength test specimen structure of the present invention;

[0024] Figure 3 It is a schematic diagram of the sample stacking structure of the present invention;

[0025] Figure 4 This is a schematic diagram of the structure for testing the wear resistance of the low-pressure cold-sprayed aluminum-based conductive layer of the present invention;

[0026] Figure 5 A schematic diagram of the microstructure of the low-pressure cold sprayed Al-Ni coating of the present invention;

[0027] Figure 6 A schematic diagram of the microstructure of the low-pressure cold sprayed Al-Ni-Al2O3 conductive coating of the present invention;

[0028] Figure 7 A schematic diagram of friction coefficients of three conductive layers of the present invention;

[0029] Figure 8 Schematic diagram of the wear weight loss of three conductive layers of the present invention;

[0030] Figure numerals: 1. bonding strength specimen; 2. coating; 3. FM1000 film; 4. mating part; 5. loading rod; 6. Si3N4 ball; 7. metallographic and friction and wear specimen; 8. specimen rotation direction. DETAILED DESCRIPTION

[0031] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below.

[0032] like Figures 1 to 8As shown, a method for preparing an aluminum-based conductive coating on the surface of a composite material, the specific steps are as follows:

[0033] S1. Preparation of powder raw materials: selecting powders according to requirements, and then fully mixing the powders, using a powder mixer, at a rotation speed of 5 rpm to 15 rpm, mixing the two powders for 30 min to 60 min, thereby obtaining the final powder raw materials for low-pressure cold spraying;

[0034] S2. Preparation of low pressure cold spray coating 2:

[0035] S21: Select carbon fiber composite material as the matrix and prepare metallographic, microhardness and resistance test specimens; select LY12 aluminum alloy as the matrix and prepare wear-resistant specimens for testing. Figure 1 , reference numeral a is the coating deposition position, and the bonding strength specimen 1 is shown in Figure 2 ;

[0036] S22: Add a top iron as support on the back of the area to be sprayed on the carbon fiber composite material to prevent deformation of the composite material, and then sandblast the area to be sprayed. After sandblasting, use compressed air to blow the surface of the sample to prevent the adhesion of sand particles and floating dust;

[0037] S23: Within 4 hours after powder mixing and within 2 hours after sandblasting, use low-pressure cold spraying process to prepare aluminum-based conductive coating 2 on the surface of the sample. During the process, use infrared thermometer to monitor the surface temperature of the part in real time, which should not be higher than 90°C;

[0038] S24: The surface of the coating 2 of the bonding strength specimen 1 is polished to a roughness of Ra0.8μm by mechanical processing, and then the bonding surface of the coating 2 of the bonding strength specimen 1 and the mating part 4 is sandblasted. Figure 3 As shown, the dual parts 4-FM1000 film 3-bonding strength sample 1 are stacked and placed in sequence, and a pressure of 5kg to 6kg is applied to both ends. Under the condition of maintaining the pressure, they are placed in an oven and finally cooled in the oven;

[0039] S25: Remove the supporting top iron on the back of the carbon fiber composite material sample, and polish the surface coating 2 of the metallographic and friction and wear sample 7 with 600 mesh, 800 mesh, 1000 mesh, and 2000 mesh sandpaper in sequence, and then polish the coating 2 with 3 μm diamond polishing liquid and 0.02 μm silicon oxide polishing liquid.

[0040] S3, coating 2 performance test:

[0041] S31. Visually inspect the surface of the low-pressure cold-sprayed aluminum-based conductive layer. The coating 2 should be free of cracks, warping, peeling or shedding.

[0042] S32. The microstructure of the low-pressure cold-sprayed aluminum-based conductive layer was observed using a scanning electron microscope, and the porosity of the coating 2 was analyzed with reference to the standard HB20195-2014 "Metallographic Inspection of Thermal Sprayed Coatings";

[0043] S33, using an automatic micro-Vickers hardness tester to measure the microhardness of the low-pressure cold-sprayed aluminum-based conductive layer;

[0044] S34. Refer to GB / T 8642-2002 "Determination of tensile bond strength of thermal spraying" standard to evaluate the bonding strength of low-pressure cold-sprayed aluminum-based conductive layer;

[0045] S35. By means of a friction and wear tester, the wear resistance of the low-pressure cold-sprayed aluminum-based conductive layer was tested by using a ball-on-disc wear tester and using Si3N4 ball 6 as a counter-wear member under a load of 10N and a linear speed of 125mm / s for 10min;

[0046] S36. With the help of BT3562A resistance measuring instrument, the resistance of the low-pressure cold-sprayed aluminum-based conductive layer was measured using a four-probe method.

[0047] The powder selection criteria in step S1 are:

[0048] Select spherical pure Al powder with a purity greater than 99%, a particle size of 5 to 38 μm, and a D50 of 14 to 16 μm;

[0049] Selecting irregularly shaped pure Ni powder with a purity greater than 99%, a particle size of 5 to 20 μm, and a D50 of 8 to 10 μm;

[0050] Irregularly shaped Al2O3 powder with a purity greater than 99%, a particle size of 10 to 30 μm, and a D50 of 20 to 24 μm is selected as the raw material.

[0051] The three powders are mixed in a ratio of 12±2wt.% Ni powder, 10±2wt.% Al2O3 powder and the remainder Al powder. By adjusting the particle size and ratio of Al, Ni and Al2O3 in the powder raw materials and the matching low-pressure cold spraying process parameters, the preparation of low-pressure cold sprayed aluminum-based conductive coating 2 on the surface of the composite material is achieved.

[0052] In the step S21, acetone is required to be used to fully clean the surface of the sample before the wear resistance test to remove various oil stains and impurities.

[0053] In the step S22, the roughness of the area to be sprayed on the surface of the carbon fiber composite material and the LY12 aluminum alloy needs to reach Ra4.0 to Ra7.0. If the local roughness does not meet the requirement, the local area can be re-sprayed.

[0054] In step S22, the process parameters of the aluminum-based conductive coating 2 are:

[0055] (1) Process gas: nitrogen with a purity of not less than 99.9%;

[0056] (2) Spraying pressure: 1.38MPa~1.59MPa;

[0057] (3) Gas heating temperature: 450℃~550℃;

[0058] (4) Powder feeding rate 10g / min~20g / min;

[0059] (5) Spraying distance: 15mm~25mm;

[0060] (6) Spraying angle: 90°±20°;

[0061] (7) Spraying line speed: 150mm / s~300mm / s.

[0062] The oven temperature in step S24 is heated to 180° C. to 190° C. as a whole and kept warm for 2 h to 2.5 h.

[0063] The low-pressure cold-sprayed Al-Ni-Al2O3 conductive coating 2 in step S32 has the advantages of high density, high hardness, high bonding strength, good wear resistance and low resistivity, so that a conductive layer of lower thickness can meet the use requirements, reducing the impact of the weight gain of the coating 2 on the flight of the aircraft, and effectively solving the problems of low density, poor bonding performance, poor wear resistance and high resistivity of the flame-sprayed aluminum layer on the surface of the composite material.

[0064] The test method of step S35 is as follows Figure 4 As shown, a loading force b is applied by a loading rod 5, reference numeral 8 is the rotation direction of the sample, and an electronic balance with an accuracy of 0.00001g is used to measure the mass of the sample before and after the friction and wear test, and the weight loss of the sample before and after the test is calculated.

[0065] In order to demonstrate the beneficial effects of the low-pressure cold sprayed aluminum-based conductive coating 2 and the powder ratio, a flame sprayed aluminum comparison group and a low-pressure cold sprayed Al-Ni coating 2 comparison group were set up.

[0066] Flame sprayed aluminum layer comparison group:

[0067] Using 3mm 1060 aluminum wire as raw material, flame spraying method, and the same base material, metallographic and microhardness, resistance test, bonding strength, and wear resistance test samples were prepared. The test results show that the porosity of the flame sprayed aluminum layer is 5%, the microhardness is 62HV, the bonding strength is less than 8MPa, and the friction coefficient is stable at 0.7. Figure 7 ; The weight loss by abrasion is 5.2 mg, see Figure 8; The flame sprayed aluminum layer with a thickness of about 0.1mm has a resistance of about 1.52mΩ.

[0068] Low-pressure cold sprayed Al-Ni coating 2 comparison group:

[0069] The same pure Al powder and pure Ni powder as those of the present invention are selected as raw materials, and the two powders are mixed in a ratio of (12±2) wt.% Ni powder and the balance Al powder. The two powders are mixed for 30min to 60min at a rotation speed of 5rpm to 15rpm using a powder mixer.

[0070] The same low-pressure cold spraying process as the present invention was used to prepare metallographic and microhardness, resistance test, bonding strength, and wear resistance test samples. Figure 5 As shown, the porosity of coating 2 is about 0.5%, the microhardness is 68HV0.1, the bonding strength reaches more than 30MPa, and the friction coefficient is stable at 0.4. Figure 7 ; Wear loss 2.7mg, see Figure 8 ; The resistance of the low-pressure cold-sprayed Al-Ni coating 2 with a thickness of about 0.10 mm is about 0.54 mΩ.

[0071] The performance test results of the low-pressure cold sprayed Al-Ni-Al2O3 conductive coating 2 of the present invention are as follows:

[0072] (1) Figure 6 This is the microstructure image of the low-pressure cold sprayed Al-Ni-Al2O3 conductive coating 2. The porosity of the coating 2 is less than 0.4%, and the density of the coating 2 is further increased, which is also slightly improved compared with the low-pressure cold sprayed Al-Ni coating 2.

[0073] (2) The microhardness of the low-pressure cold sprayed Al-Ni-Al2O3 conductive coating 2 is about 77 HV, which is significantly greater than that of the flame sprayed aluminum layer and the low-pressure cold sprayed Al-Ni coating 2.

[0074] (3) The bonding strength of the low-pressure cold sprayed Al-Ni-Al2O3 conductive coating 2 reaches above 35 MPa, and the bonding performance between the coating 2 and the substrate is significantly improved.

[0075] (4) The friction coefficient of the low-pressure cold sprayed Al-Ni-Al2O3 conductive coating 2 is stable at 0.38. Figure 7 , compared with the flame sprayed aluminum layer and the low-pressure cold sprayed Al-Ni coating 2, the friction coefficient of the coating 2 is lower.

[0076] (5) The wear weight loss of the low-pressure cold sprayed Al-Ni-Al2O3 conductive coating 2 is 2.2 mg. Figure 8 Compared with the flame sprayed aluminum layer and the low-pressure cold sprayed Al-Ni coating 2, the coating 2 has a lower wear rate and better wear resistance.

[0077] (6) The low-pressure cold sprayed Al-Ni-Al2O3 conductive coating 2 with a thickness of about 0.10 mm has a resistance of about 0.56 mΩ.

[0078] The present invention mixes Al-Ni-Al2O3 powder in a certain ratio and cooperates with a suitable low-pressure cold spraying process to achieve the preparation of low-pressure cold sprayed aluminum-based conductive coating 2 on the surface of the composite material. The specific beneficial effects are as follows:

[0079] (1) Compared with the flame-sprayed aluminum layer on the surface of the traditional composite material, the low-pressure cold-sprayed Al-Ni-Al2O3 conductive coating 2 has a high density. The addition of Ni and Al2O3 powders effectively improves the hardness, bonding strength, wear resistance and depositability of the coating 2; Note: Using this process, the low-pressure cold-sprayed pure Al coating 2 cannot be deposited on the composite material, and the low-pressure cold-sprayed Al-Ni-Al2O3 conductive coating 2 has a lower resistivity. A conductive layer of lower thickness can meet the use requirements, reducing the impact of the weight gain of the coating 2 on the flight of the aircraft.

[0080] (2) Compared with the low-pressure cold-sprayed Al-Ni coating 2 on the surface of the composite material, the resistivity of the low-pressure cold-sprayed Al-Ni-Al2O3 conductive coating 2 is slightly increased, but the difference is very small and can also meet the conductive requirements of the composite surface without causing an increase in the thickness of the conductive layer. In addition, the hardness, bonding strength and wear resistance of the Al-Ni-Al2O3 conductive coating 2 are higher, which can prevent accidental damage to the conductive layer and increase the reliability of the conductive layer. Therefore, the low-pressure cold-sprayed Al-Ni-Al2O3 conductive coating 2 is preferred.

[0081] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing an aluminum-based conductive coating on a composite material surface, characterized in that: The specific steps are as follows: S1. Preparation of powder raw materials: selecting powders according to requirements, and then fully mixing the powders, using a powder mixer, at a rotation speed of 5 rpm to 15 rpm, mixing the two powders for 30 min to 60 min, thereby obtaining the final powder raw materials for low-pressure cold spraying; S2. Preparation of low pressure cold spray coating (2): S21: Select carbon fiber composite material as the matrix and prepare metallographic, microhardness and resistance test specimens; select LY12 aluminum alloy as the matrix and prepare wear resistance test; S22: Add a top iron as support on the back of the area to be sprayed on the carbon fiber composite material, perform sandblasting on the area to be sprayed, and after sandblasting, use compressed air to blow the surface of the sample; S23: Within 4 hours after powder mixing and within 2 hours after sandblasting, an aluminum-based conductive coating (2) is prepared on the surface of the sample by a low-pressure cold spraying process. During the process, an infrared thermometer is used to monitor the surface temperature of the part in real time, and the temperature is not higher than 90°C; S24: The coating (2) surface of the bonding strength specimen (1) is polished to a roughness of Ra 0.8 μm by mechanical processing, and the coating (2) surface of the bonding strength specimen (1) and the bonding surface of the mating piece (4) are sandblasted, and the mating piece (4)-FM1000 film (3)-bonding strength specimen (1) are stacked and placed in sequence, and a pressure of 5 kg to 6 kg is applied to both ends. The specimens are placed in an oven while maintaining the pressure, and finally cooled in the oven; S25: removing the supporting top iron on the back of the carbon fiber composite material sample, and polishing the surface coating (2) of the metallographic and friction and wear samples (7) with 600 mesh, 800 mesh, 1000 mesh, and 2000 mesh sandpaper in sequence, and then polishing the coating (2) with 3 μm diamond polishing liquid and 0.02 μm silicon oxide polishing liquid; S3. Coating (2) performance test: S31. Inspect the surface of the low-pressure cold-sprayed aluminum-based conductive layer by visual inspection. The coating (2) should be free of cracks, warping, peeling or shedding; S32, observing the microstructure of the low-pressure cold-sprayed aluminum-based conductive layer using a scanning electron microscope, and analyzing the porosity of the coating (2) with reference to relevant standards; S33, using an automatic micro-Vickers hardness tester to measure the microhardness of the low-pressure cold-sprayed aluminum-based conductive layer; S34. Evaluate the bonding strength of the low-pressure cold-sprayed aluminum-based conductive layer with reference to the relevant standards; S35. Using a friction and wear tester, the wear resistance of the low-pressure cold-sprayed aluminum-based conductive layer is tested by using a ball-on-disc wear tester with Si3N4 balls (6) as the wear parts under a load of 10N and a linear speed of 125mm / s for 10min. S36. With the help of BT3562A resistance measuring instrument, the resistance of the low-pressure cold-sprayed aluminum-based conductive layer was measured using a four-probe method.

2. The method for preparing an aluminum-based conductive coating on a composite material surface according to claim 1, characterized in that: The powder selection criteria in step S1 are: Select spherical pure Al powder with a purity greater than 99%, a particle size of 5 to 38 μm, and a D50 of 14 to 16 μm; Selecting irregularly shaped pure Ni powder with a purity greater than 99%, a particle size of 5 to 20 μm, and a D50 of 8 to 10 μm; Irregularly shaped Al2O3 powder with a purity greater than 99%, a particle size of 10 to 30 μm, and a D50 of 20 to 24 μm is selected as the raw material.

3. The method for preparing an aluminum-based conductive coating on a composite material surface according to claim 2, characterized in that: The three powders are mixed in a ratio of 12±2wt.% Ni powder, 10±2wt.% Al2O3 powder and the balance Al powder.

4. The method for preparing an aluminum-based conductive coating on a composite material surface according to claim 1, characterized in that: In the step S21, acetone is required to be used to fully clean the surface of the sample before the wear resistance test to remove various oil stains and impurities.

5. The method for preparing an aluminum-based conductive coating on a composite material surface according to claim 1, characterized in that: In the step S22, the roughness of the area to be sprayed on the surface of the carbon fiber composite material and the LY12 aluminum alloy needs to reach Ra4.0 to Ra7.

0. If the local roughness does not meet the requirement, the local area can be re-sprayed.

6. The method for preparing an aluminum-based conductive coating on a composite material surface according to claim 1, characterized in that: In the step S22, the process parameters of the aluminum-based conductive coating (2) are: (1) Process gas: nitrogen with a purity of not less than 99.9%; (2) Spraying pressure: 1.38MPa~1.59MPa; (3) Gas heating temperature: 450℃~550℃; (4) Powder feeding rate 10g / min~20g / min; (5) Spraying distance: 15mm~25mm; (6) Spraying angle: 90°±20°; (7) Spraying line speed: 150mm / s~300mm / s.

7. The method for preparing an aluminum-based conductive coating on a composite material surface according to claim 1, characterized in that: The oven temperature in step S24 is heated to 180° C. to 190° C. as a whole and kept warm for 2 h to 2.5 h.

8. The method for preparing an aluminum-based conductive coating on a composite material surface according to claim 1, characterized in that: The test method of step S35 requires using an electronic balance with an accuracy of 0.00001g to measure the mass of the sample before and after the friction and wear test, and calculating the weight loss of the sample before and after the test.

Citation Information

Patent Citations

  • Preparation method of high-performance low-pressure cold spraying pure aluminum coating

    CN116904982A

  • Method for application of heat-protective and conductive coating on carbon fibres and fabrics

    RU2511146C1

  • Fiber-Reinforced Copper-Based Brake Pad for High-speed railway train, and Preparation and Friction Braking Performance Thereof

    US20200208701A1

  • Cold sprayed electrical circuits and methods thereof

    US20230279554A1

Cited By

  • Preparation method of 6101 aluminum alloy composite plate for new energy automobile conducting bar

    CN121696247A

  • Preparation method of 6101 aluminum alloy composite plate for new energy automobile conductive bar

    CN121696247B