Aluminum-zirconium composite spinning solution, precursor fiber, and preparation method of zirconium oxide-aluminum oxide composite short fiber
The aluminum-zirconium composite spinning solution was prepared by the sol-gel method and dry spinning chopped technology was used to solve the problems of uneven fiber diameter and environmental pollution in the preparation of zirconium-alumina composite fibers, and achieve efficient and environmentally friendly spinning. The preparation of zirconia-alumina composite short fibers improves the performance of the fiber and simplifies the process.
Patent Information
- Application Number
- CN202211435557.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-11-16
AI Technical Summary
The existing zirconia-alumina composite fiber preparation method has problems such as uneven fiber diameter, many defects and environmental pollution, and needs to be improved to improve the efficiency and environmental protection of the preparation process.
Aluminum hydroxide, zirconium hydroxide, organic carboxylic acid, yttrium acetate and boric acid are used as raw materials to prepare the aluminum-zirconium composite spinning liquid through the sol-gel method. After vacuum degassing and spinning, it is chopped by dry spinning. Precursor fibers are prepared using technology and heat-treated in a muffle furnace to obtain zirconia-alumina composite short fibers.
It achieves uniformity of fiber diameter and length, reduces process complexity, avoids the generation of Cl-, SO42-, NO3- plasma, reduces environmental pollution, and improves the toughness and density of the fiber.
Smart Images

Figure CN115896980B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite fibers, and in particular to a method for preparing an aluminum-zirconium composite spinning solution, a precursor fiber, and a zirconium oxide-aluminum oxide composite short fiber. Background Art
[0002] Zirconia-alumina composite fibers not only have high temperature resistance, but also can make full use of zirconium oxide to play the role of phase change toughening and microcrack toughening, increasing the toughness and strength of alumina. Therefore, the performance of zirconia-alumina composite fibers is better than that of pure alumina or zirconia ceramic fibers, its use temperature is higher than that of alumina ceramic fibers, and its bending strength and fracture toughness are higher than those of zirconia ceramic fibers. In view of the excellent performance of zirconia-alumina composite fibers, researchers have carried out extensive research. For example, patent number CN102465357B reports a method for preparing polycrystalline zirconia fibers and zirconia / alumina composite fibers, which uses zirconium carbonate and hydrochloric acid as raw materials, refluxes to obtain polyhydroxy zirconium chloride sol; then adds aluminum sol, phase stabilizer, grain growth inhibitor and water-soluble polymer additive, and obtains zirconium-aluminum composite spinning solution by vacuum distillation, and makes gel fiber by centrifugal spinning or blow spinning, and obtains zirconia / alumina composite fiber by heat treatment. For example, the patent number CN111074379B reports a method for preparing alumina-zirconia composite short fibers, in which aluminum powder, hydrochloric acid and water are heated and refluxed to obtain a polyaluminum chloride sol, zirconium oxychloride solution is added and mixed to obtain zirconium aluminum gel, which is spun into fibers to obtain precursor fibers, and heat-treated to obtain alumina-zirconia composite short fibers. For example, Fu Chao et al. used aluminum powder, hydrochloric acid, zirconium acetate and zirconium oxychloride as raw materials, polyvinyl alcohol as a spinning aid, and used the sol-gel method to prepare alumina-zirconia precursor fiber spinning solution, and prepared gel fibers with the help of a high-speed centrifugal spinning machine (see: Materials Guide B2015, 29, 68). The above three methods all use centrifugal spinning or blow spinning technology, and the prepared fibers have uneven diameters and many defects. Patent number CN107266081B reports a method for preparing alumina-zirconia composite ceramic continuous fibers, which uses alumina sol containing Al13 colloid particles, γ-AlOOH nano-dispersion, zirconium acetate, yttrium nitrate and polyvinyl alcohol (PVA) to prepare a spinnable precursor sol, uses dry spinning technology to prepare gel fibers, and obtains alumina-zirconia composite ceramic continuous fibers after heat treatment. In this method, alumina sol is prepared with aluminum powder and aluminum chloride, aluminum sulfate, aluminum nitrate, etc. Cl - 、SO4 2- 、NO3 - The presence of plasma causes great environmental pollution during the fiber heat treatment process. The above preparation methods all have certain problems and defects, so the preparation methods need further improvement and development. Summary of the invention
[0003] The present invention provides an aluminum-zirconium composite spinning solution, a precursor fiber, a zirconium oxide-aluminum oxide composite short fiber and a preparation method, and the specific scheme is as follows:
[0004] A method for preparing an aluminum-zirconium composite spinning solution. The aluminum-zirconium composite spinning solution is prepared by a sol-gel method using aluminum hydroxide, zirconium hydroxide, organic carboxylic acid, yttrium acetate and boric acid as raw materials.
[0005] Furthermore, the organic carboxylic acid and water are mixed and then aluminum hydroxide is added. After the first condensation reflux is carried out at 70-95°C, zirconium hydroxide is added and the condensation reflux is continued. After cooling and filtering, a carboxylate aluminum zirconium sol is obtained. Yttrium acetate, boric acid and polyvinyl alcohol are added to the carboxylate aluminum zirconium sol, and the aluminum zirconium composite spinning solution is obtained by reduced pressure distillation.
[0006] Furthermore, the molar ratio of aluminum hydroxide to organic carboxylic acid is 1:1-2.5; the molar ratio of aluminum hydroxide to water is 1:10-20; the molar ratio of aluminum hydroxide to zirconium hydroxide is 10-25:1; the molar ratio of zirconium hydroxide to yttrium acetate is 15-50:1; and the molar ratio of aluminum hydroxide to boric acid is 28-108:1.
[0007] Furthermore, the amount of polyvinyl alcohol added is 0.2-1.4 wt % of the total mass of the raw materials.
[0008] Furthermore, the organic carboxylic acid is one or more of formic acid, acetic acid, oxalic acid, malonic acid, and citric acid.
[0009] Furthermore, the first condensation reflux time is 8-10 hours, and the time for adding zirconium hydroxide to continue condensation reflux is 10-30 minutes.
[0010] Furthermore, the temperature of the reduced pressure distillation is 40-50° C., and the distillation is performed to a viscosity of 300-800 Pa·s.
[0011] An aluminum-zirconium composite spinning solution is prepared by the above-mentioned aluminum-zirconium composite spinning solution preparation method.
[0012] A method for preparing a precursor fiber comprises the steps of vacuum degassing the aluminum-zirconium composite spinning solution, spinning the spinning solution, and obtaining the precursor fiber after drawing, dropping and chopping.
[0013] Further, the spinning solution is spun under the conditions of an ambient temperature of 20-30° C. and a relative humidity of 15-35%.
[0014] Furthermore, a metering pump is used to spin the spinning solution, and the flow rate of the metering pump is 30-60cc / min.
[0015] Furthermore, after drawing, dropping and short cutting, precursor fibers with a diameter of 12-20 microns and a length of 1-50 cm are obtained.
[0016] Furthermore, the spinneret used for spinning has an aperture of 0.1-0.12 mm and a number of holes of 1000-2000.
[0017] A precursor fiber is prepared by using a precursor fiber preparation method.
[0018] A method for preparing zirconia-alumina composite short fibers, comprising placing the above-mentioned precursor fibers in a muffle furnace, first slowly heating the temperature to 100-150°C, and then keeping the temperature at this temperature for 0.5-1h; then slowly heating the temperature to 600-700°C, and keeping the temperature at this temperature for 0.5-1h; and finally heating the temperature to 1200-1400°C, and keeping the temperature at this temperature for 0.5-2h to obtain zirconia-alumina composite short fibers.
[0019] Further, the temperature is increased to 100-150°C at a rate of 0.1-1.0°C / min, the temperature is increased to 600-700°C at a rate of 0.5-3.0°C / min, and the temperature is increased to 1200-1400°C at a rate of 5-10°C / min.
[0020] A zirconia-alumina composite short fiber is prepared by using the above-mentioned zirconia-alumina composite short fiber preparation method.
[0021] Due to the adoption of the above technical solution, the beneficial technical effects of the present invention are:
[0022] 1. The present invention uses zirconium hydroxide, aluminum hydroxide and organic carboxylic acid as main raw materials and does not contain Cl - 、SO4 2- 、NO3 - Plasma, no substances that affect the environment are produced during the production process.
[0023] 2. Compared with the existing centrifugal spinning or blowing technology, the dry spinning and chopping technology adopted by the present invention can chop the precursor fibers into any length within 1-50 cm according to the needs, and the diameter and length of the fibers after heat treatment are more uniform.
[0024] 3. The present invention directly uses aluminum hydroxide and zirconium hydroxide as main raw materials to prepare aluminum-zirconium composite spinning solution. Compared with the prior art of separately preparing aluminum sol and zirconium sol, the process complexity is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a picture of the zirconia-alumina composite short fiber prepared in Example 3 of the present invention;
[0026] Figure 2This is a SEM image of the zirconia-alumina composite short fibers of Example 3 of the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] The present invention provides a method for preparing an aluminum-zirconium composite spinning solution, wherein the aluminum-zirconium composite spinning solution is prepared by a sol-gel method using aluminum hydroxide, zirconium hydroxide, organic carboxylic acid, yttrium acetate and boric acid as raw materials. The present invention uses zirconium hydroxide, aluminum hydroxide and organic carboxylic acid as main raw materials and does not contain Cl - 、SO4 2- 、NO3 - Plasma, no substances that affect the environment are produced during the production process.
[0029] Specifically, after mixing organic carboxylic acid and water, aluminum hydroxide is added, and condensation reflux is performed at 70-95°C for 8-10h, and then zirconium hydroxide is added, and condensation reflux is continued for 10-30min; carboxylic acid aluminum zirconium sol is obtained after cooling and filtering, and yttrium acetate, boric acid and polyvinyl alcohol are added to the carboxylic acid aluminum zirconium sol, and aluminum zirconium composite spinning solution is obtained by reduced pressure distillation. Boric acid is added in the present invention to reduce grain growth, improve the toughness of the fiber, and can also reduce the crystal phase transition temperature and the heat treatment temperature. Yttrium acetate is added to stabilize zirconium oxide in the tetragonal phase to avoid fiber volume cracking during heat treatment, and can also inhibit grain growth and improve the density of the fiber. The temperature of condensation reflux is 70-95°C. When the temperature of condensation reflux is lower than 70°C, aluminum hydroxide and zirconium oxide do not react with organic carboxylic acid, and a transparent and spinnable spinning solution cannot be obtained. When the temperature of condensation reflux exceeds 95°C, a white precipitate will be produced, and it cannot be distilled to form a spinning solution after filtration. Condensation reflux has the function of concentration and purification. In the preparation process of aluminum-zirconium composite spinning solution, carboxylate aluminum-zirconium sol is obtained after two condensation refluxes. The selection of the time of adding zirconium hydroxide is very important. The product of the reaction of zirconium hydroxide and organic carboxylic acid has poor thermal stability. If aluminum hydroxide and zirconium hydroxide are added at the same time, white precipitate will be produced and spinning solution cannot be formed.
[0030] In a specific embodiment, the molar ratio of aluminum hydroxide to organic carboxylic acid is 1:1-2.5; when the molar ratio of aluminum hydroxide to organic carboxylic acid is within the range of 1:1-2.5, aluminum hydroxide reacts with organic carboxylic acid to generate linear Al oligomers, which is also the key to the spinnability of the spinning solution. Further preferably, the molar ratio of aluminum hydroxide to organic carboxylic acid is 1:2.
[0031] The molar ratio of aluminum hydroxide to water is 1:10-20. When the molar ratio of aluminum hydroxide to water is too high or too low, the pH of the aluminum hydroxide solution will be affected, thereby affecting the reaction of aluminum hydroxide with the organic carboxylic acid. Further preferably, the molar ratio of aluminum hydroxide to water is 1:12.
[0032] The molar ratio of aluminum hydroxide to zirconium hydroxide is 10-25:1; this ratio corresponds to the amount of zirconium hydroxide added, and the ratio of zirconium oxide to aluminum oxide in the final fiber. Different ratios of zirconium oxide to aluminum oxide will lead to inconsistent mechanical properties or thermal properties of the fiber. After experimental verification, when the molar ratio of aluminum hydroxide to zirconium hydroxide is 18:1, the fiber performance is the best.
[0033] The molar ratio of zirconium hydroxide to yttrium acetate is 15-50:1; the molar ratio of zirconium hydroxide to yttrium acetate affects the amount of yttrium acetate added, yttrium acetate is a stabilizer of zirconium oxide crystal phase, and its amount affects the phase change stability of tetragonal zirconium oxide in the fiber; too much or too little yttrium acetate does not play the role of stabilizer. Preferably, the molar ratio of zirconium hydroxide to yttrium acetate is 16:1.
[0034] The molar ratio of aluminum hydroxide to boric acid is 28-108:1. When the amount of boric acid is too high, the mechanical properties of the final fiber are affected; when the amount of boric acid is too low, it cannot act as a sintering aid. Preferably, the molar ratio of aluminum hydroxide to boric acid is 36:1.
[0035] Specifically, the amount of polyvinyl alcohol added is 0.2-1.4wt% of the total mass of the raw materials. Polyvinyl alcohol is a spinning aid, which is beneficial to spinning. Too little polyvinyl alcohol cannot improve the spinnability of the spinning solution; too much polyvinyl alcohol will cause a large number of hole defects in the fiber. The optimal amount of polyvinyl alcohol added is 1.0wt%.
[0036] Specifically, the organic carboxylic acid is one or more of formic acid, acetic acid, oxalic acid, malonic acid, and citric acid. The organic carboxylic acid reacts with aluminum hydroxide and zirconium hydroxide to produce uniform and transparent aluminum zirconium carboxylate sol, among which formic acid, oxalic acid, and acetic acid have the best effect.
[0037] Specifically, the vacuum distillation temperature is 40-50°C, and the viscosity is distilled to 300-800 Pa·s. When the vacuum distillation temperature is lower than 40°C, the reaction efficiency is low, which affects the stability of the spinning solution; when the vacuum distillation temperature is higher than 50°C, the gelation of the spinning solution is accelerated, and a transparent and spinnable spinning solution cannot be obtained.
[0038] The viscosity of the spinning solution is measured by a rotational rheometer. As an indicator, the viscosity can indirectly indicate the spinnability of the spinning solution. For spinning solutions that are not within this viscosity range, it is impossible to prepare short fibers using the dry spinning and chopped process.
[0039] The present invention also provides a method for preparing a precursor fiber, wherein the aluminum-zirconium composite spinning solution is subjected to vacuum degassing, and the spinning solution is spun under the conditions of an ambient temperature of 20-30°C and a relative humidity of 15-35%. The spinning solution is spun using a metering pump, the flow rate of the metering pump is 30-60cc / min, and the precursor fiber is obtained after drawing, dropping and short cutting. After drawing, dropping and short cutting, the precursor fiber with a diameter of 12-20 microns and a length of 1-50cm is obtained. Specifically, the precursor fiber after drawing is cut by a frequency-adjustable scissors before falling onto the disc. The fiber diameter can be adjusted by adjusting the drawing rate, and the fiber length can be adjusted by adjusting the scissors frequency.
[0040] The spinneret used for spinning has an aperture of 0.1-0.12mm and 1000-2000 holes. If the aperture of the spinneret is less than 0.1mm, the spinning pressure will be extremely high, which cannot be met by current equipment; if the aperture is greater than 0.12mm, the resulting fiber diameter will be coarse. The function of the metering pump is to input the spinning solution into the spinneret at a constant pressure and a flow rate of 30-60cc / min can ensure uniform spinning of the filaments.
[0041] The above-mentioned precursor fiber is used to prepare zirconia-alumina composite short fibers. The specific method is to place the precursor fiber in a muffle furnace, heat it to 100-150°C at a rate of 0.1-1.0°C / min, and keep it at this temperature for 0.5-1h; then heat it to 600-700°C at a rate of 0.5-3.0°C / min, and keep it at this temperature for 0.5-1h; finally heat it to 1200-1400°C at a rate of 5-10°C / min, and keep it at this temperature for 0.5-2h to obtain zirconia-alumina composite short fibers. The precursor fiber is subjected to high-temperature heat treatment. After three heating and heat preservation, the precursor fiber is subjected to uniform diameter and length of boron-containing zirconia-alumina composite short fibers. The three heating processes use different heating rates. The first stage is mainly to remove the solvent in the fiber, which requires slow heating. The second stage is the ceramicization process, which mainly removes organic matter in the fiber, and the heating rate is moderate. The third stage is crystallization, which is mainly the transformation of the crystal form, and requires rapid heating.
[0042] The morphology of zirconia-alumina composite short fibers can be referred to Figure 1 and Figure 2 , Figure 1 and Figure 2 Provided are photos and scanned images of zirconia-alumina composite short fibers (taking Example 3 as an example).
[0043] The present invention will be further described below in conjunction with the embodiments.
[0044] Example 1
[0045] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0046] (1) Preparation of spinning solution
[0047] Fully dissolve 6 mol of oxalic acid, 1.5 mol of acetic acid and 60 mol of water and mix them evenly, then add 3 mol of aluminum hydroxide; condense and reflux at 95°C for 10 hours; add 0.3 mol of zirconium hydroxide; continue condensing and reflux for 30 minutes; cool and filter to obtain a uniform and transparent carboxylate aluminum zirconium sol; add 0.02 mol of yttrium acetate, 0.15 mol of boric acid and 0.99 mol of polyvinyl alcohol to the above carboxylate aluminum zirconium sol, and distill under reduced pressure at 50°C to a viscosity of 800 Pa·s to obtain a spinnable aluminum-zirconium composite spinning solution.
[0048] (2) Preparation of precursor fibers
[0049] The aluminum-zirconium composite spinning solution prepared in step (1) is poured into a material tank and vacuum degassed for 10 minutes. Under the conditions of an ambient temperature of 30°C and a relative humidity of 35%, the spinning solution is spun using a metering pump with a flow rate of 60cc / min. The precursor fibers are obtained through a drawing and cutting device.
[0050] (3) High temperature heat treatment
[0051] The precursor fiber prepared in step (2) is placed in a muffle furnace, and the temperature is increased to 150°C at a rate of 1°C / min, and kept at this temperature for 1 hour; then the temperature is increased to 700°C at a rate of 3°C / min, and kept at this temperature for 1 hour; finally, the temperature is increased to 1400°C at a rate of 10°C / min, and kept at this temperature for 2 hours to obtain boron-containing zirconia-alumina composite short fibers with uniform diameter and length.
[0052] Example 2
[0053] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0054] (1) Preparation of spinning solution
[0055] 3 mol of oxalic acid and 30 mol of water are fully dissolved and mixed uniformly, and then 3 mol of aluminum hydroxide is added; after condensation and reflux at 70°C for 8 hours, 0.12 mol of zirconium hydroxide is added; condensation and reflux are continued for 10 minutes; cooling and filtering are performed to obtain a uniform and transparent aluminum zirconium carboxylate sol; 0.0024 mol of yttrium acetate, 0.028 mol of boric acid and 0.07 mol of polyvinyl alcohol are added to the above aluminum zirconium carboxylate sol, and vacuum distillation is performed at 40°C to a viscosity of 300 Pa·s to obtain an aluminum zirconium composite spinning solution with spinnability;
[0056] (2) Preparation of precursor fibers
[0057] The aluminum-zirconium composite spinning solution prepared in step (1) is poured into a material tank and vacuum degassed for 5 minutes. Under the conditions of an ambient temperature of 20°C and a relative humidity of 15%, the spinning solution is spun using a metering pump with a flow rate of 30cc / min. The precursor fibers are obtained through a drawing and cutting device.
[0058] (3) High temperature heat treatment
[0059] The precursor fiber prepared in step (2) is placed in a muffle furnace, and the temperature is increased to 100°C at a rate of 0.1°C / min, and kept at this temperature for 0.5h; then the temperature is increased to 600°C at a rate of 0.5°C / min, and kept at this temperature for 0.5h; finally, the temperature is increased to 1200°C at a rate of 5°C / min, and kept at this temperature for 0.5h, to obtain boron-containing zirconia-alumina composite short fibers with uniform diameter and length.
[0060] Example 3
[0061] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0062] (1) Preparation of spinning solution
[0063] 2 mol of formic acid, 2 mol of acetic acid, 2 mol of oxalic acid and 36 mol of water are fully dissolved and mixed uniformly, and then 3 mol of aluminum hydroxide is added; after condensation and reflux at 85°C for 9 hours, 0.17 mol of zirconium hydroxide is added; condensation and reflux are continued for 20 minutes; cooling and filtering are performed to obtain a uniform and transparent aluminum zirconium carboxylate sol; 0.01 mol of yttrium acetate, 0.083 mol of boric acid and 0.45 mol of polyvinyl alcohol are added to the above aluminum zirconium carboxylate sol, and vacuum distillation is performed at 40°C to a viscosity of 300 Pa·s to obtain an aluminum zirconium composite spinning solution with spinnability;
[0064] (2) Preparation of precursor fibers
[0065] The aluminum-zirconium composite spinning solution prepared in step (1) is poured into a material tank and vacuum degassed for 8 minutes. Under the conditions of an ambient temperature of 25°C and a relative humidity of 20%, the spinning solution is spun using a metering pump with a flow rate of 50cc / min. The precursor fibers are obtained through a drawing and cutting device.
[0066] (3) High temperature heat treatment
[0067] The precursor fiber prepared in step (2) is placed in a muffle furnace, and the temperature is increased to 125°C at a rate of 0.5°C / min, and kept at this temperature for 0.75h; then the temperature is increased to 650°C at a rate of 2°C / min, and kept at this temperature for 0.75h; finally, the temperature is increased to 1300°C at a rate of 8°C / min, and kept at this temperature for 1h to obtain boron-containing zirconia-alumina composite short fibers with uniform diameter and length.
[0068] Example 4
[0069] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0070] (1) Preparation of spinning solution
[0071] 5.9 mol of oxalic acid, 1.6 mol of acetic acid and 42 mol of water are fully dissolved and mixed uniformly, and then 3 mol of aluminum hydroxide is added; after condensation and reflux at 70°C for 10 hours, 0.3 mol of zirconium hydroxide is added; condensation and reflux are continued for 10 minutes; cooling and filtering are performed to obtain a uniform and transparent aluminum zirconium carboxylate sol; 0.02 mol of yttrium acetate, 0.036 mol of boric acid and 0.41 mol of polyvinyl alcohol (PVA) are added to the above aluminum zirconium carboxylate sol, and vacuum distilled at 40°C to a viscosity of 450 Pa·s to obtain an aluminum zirconium composite spinning solution with spinnability;
[0072] (2) Preparation of precursor fibers
[0073] The aluminum-zirconium composite spinning solution prepared in step (1) was poured into a material tank and vacuum degassed for 5 minutes. Under the conditions of an ambient temperature of 20°C and a relative humidity of 15%, the spinning solution was spun using a metering pump with a flow rate of 60cc / min. After a drawing and cutting device, a precursor fiber with a diameter of 15 microns and a length of 1 cm was obtained.
[0074] (3) High temperature heat treatment
[0075] The precursor fiber prepared in step (2) is placed in a muffle furnace, and the temperature is increased to 100°C at a rate of 0.1°C / min, and kept at this temperature for 0.5h; then the temperature is increased to 600°C at a rate of 0.5°C / min, and kept at this temperature for 0.5; finally, the temperature is increased to 1200°C at a rate of 5°C / min, and kept at this temperature for 2h to obtain boron-containing zirconia-alumina composite short fibers with uniform diameter and length.
[0076] Example 5
[0077] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0078] (1) Preparation of spinning solution
[0079] 0.4 mol of formic acid, 1.4 mol of oxalic acid, 1.6 mol of citric acid and 30 mol of water are fully dissolved and mixed uniformly, and then 3 mol of aluminum hydroxide is added; after condensation and reflux at 95°C for 8 hours, 0.12 mol of zirconium hydroxide is added; condensation and reflux are continued for 30 minutes; cooling and filtering are performed to obtain a uniform and transparent aluminum zirconium carboxylate sol; 0.008 mol of yttrium acetate, 0.083 mol of boric acid and 0.08 mol of polyvinyl alcohol (PVA) are added to the above aluminum zirconium carboxylate sol, and vacuum distilled at 50°C to a viscosity of 800 Pa·s to obtain an aluminum zirconium composite spinning solution with spinnability;
[0080] (2) Preparation of precursor fibers
[0081] The aluminum-zirconium composite spinning solution prepared in step (1) was poured into a material tank and vacuum degassed for 10 minutes. Under the conditions of an ambient temperature of 30°C and a relative humidity of 35%, the spinning solution was spun using a metering pump with a flow rate of 30cc / min. After the drawing and cutting device, a precursor fiber with a diameter of 20 microns and a length of 50 cm was obtained.
[0082] (3) High temperature heat treatment
[0083] The precursor fiber prepared in step (2) is placed in a muffle furnace, and the temperature is increased to 150°C at a rate of 1.0°C / min, and kept at this temperature for 1 hour; then the temperature is increased to 700°C at a rate of 3.0°C / min, and kept at this temperature for 1 hour; finally, the temperature is increased to 1400°C at a rate of 10°C / min, and kept at this temperature for 0.5 hour, to obtain boron-containing zirconia-alumina composite short fibers with uniform diameter and length.
[0084] Example 6
[0085] A method for preparing boron-containing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0086] (1) Preparation of spinning solution
[0087] 1.6 mol of formic acid, 1.6 mol of acetic acid, 4.28 mol of malonic acid and 60 mol of water are fully dissolved and mixed uniformly, and then 3 mol of aluminum hydroxide is added; after condensation and reflux at 85°C for 9 hours, 0.24 mol of zirconium hydroxide is added; condensation and reflux are continued for 20 minutes; cooling and filtering are performed to obtain a uniform and transparent aluminum zirconium carboxylate sol; 0.012 mol of yttrium acetate, 0.106 mol of boric acid and 0.54 mol of polyvinyl alcohol (PVA) are added to the above aluminum zirconium carboxylate sol, and vacuum distilled at 45°C to a viscosity of 300 Pa·s to obtain an aluminum zirconium composite spinning solution with spinnability;
[0088] (2) Preparation of precursor fibers
[0089] The aluminum-zirconium composite spinning solution prepared in step (1) was poured into a material tank and vacuum degassed for 8 minutes. Under the conditions of an ambient temperature of 26°C and a relative humidity of 22%, the spinning solution was spun using a metering pump with a flow rate of 40cc / min. After the drawing and cutting device, a precursor fiber with a diameter of 16 microns and a length of 30 cm was obtained.
[0090] (3) High temperature heat treatment
[0091] The precursor fiber prepared in step (2) is placed in a muffle furnace, and the temperature is increased to 120°C at a rate of 0.6°C / min, and kept at this temperature for 0.6h; then the temperature is increased to 600°C at a rate of 1.0°C / min, and kept at this temperature for 0.5h; finally, the temperature is increased to 1300°C at a rate of 10°C / min, and kept at this temperature for 2h to obtain boron-containing zirconia-alumina composite short fibers with uniform diameter and length.
[0092] Comparative Example 1
[0093] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0094] Other conditions were the same as those in Example 3, except that zirconium hydroxide and aluminum hydroxide were added simultaneously. A white precipitate was produced, which could be distilled after filtration to form a spinning solution, but the spinnability was poor.
[0095] Comparative Example 2
[0096] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0097] The other conditions are the same as those in Example 3, except that: 4 mol formic acid, 4 mol acetic acid, 4 mol malonic acid and 75 mol water are fully dissolved and mixed, and then 3 mol aluminum hydroxide is added; after condensation and reflux at 85°C for 9 hours; 0.37 mol zirconium hydroxide is added; condensation and reflux are continued for 20 minutes; cooling and filtration are performed to obtain a uniform and transparent carboxylate aluminum zirconium sol; 0.04 mol yttrium acetate, 0.25 mol boric acid and 1.2 mol polyvinyl alcohol are added to the above carboxylate aluminum zirconium sol, and the aluminum zirconium composite spinning solution with spinnability is obtained by vacuum distillation at 40°C to a viscosity of 300 Pa·s. The prepared spinning solution is transparent, but the spinnability is poor. It can be seen from this that too much organic carboxylic acid is not conducive to the synthesis of the spinning solution.
[0098] Comparative Example 3
[0099] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0100] The other conditions are the same as those in Example 3, except that: 1 mol of formic acid, 0.5 mol of acetic acid, 0.5 mol of malonic acid and 20 mol of water are fully dissolved and mixed, and then 3 mol of aluminum hydroxide is added; after condensation and reflux at 85°C for 9 hours; 0.1 mol of zirconium hydroxide is added; condensation and reflux are continued for 20 minutes; cooling and filtration are performed to obtain a uniform and transparent carboxylate aluminum zirconium sol; 0.0015 mol of yttrium acetate, 0.02 mol of boric acid and 0.05 mol of polyvinyl alcohol are added to the above carboxylate aluminum zirconium sol, and vacuum distillation is performed at 40°C to a viscosity of 300 Pa·s to obtain a spinnable aluminum zirconium composite spinning solution. The prepared spinning solution is transparent, but the spinnability is poor. It can be seen from this that too little organic carboxylic acid is not conducive to the synthesis of the spinning solution.
[0101] Comparative Example 4
[0102] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0103] The other conditions were the same as those in Example 3, except that the condensation reflux temperature was 120° C. A large amount of white precipitate was produced, which could not be distilled to form a spinning solution after filtration. It can be seen that a too high condensation reflux temperature is not conducive to the reaction of aluminum hydroxide and zirconium hydroxide with organic carboxylic acid.
[0104] Comparative Example 5
[0105] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0106] The other conditions were the same as those in Example 3, except that the condensation reflux temperature was 60° C. A large amount of white precipitate was produced, which could not be distilled to form a spinning solution after filtration. It can be seen that a too low condensation reflux temperature is not conducive to the reaction of aluminum hydroxide and zirconium hydroxide with organic carboxylic acid.
[0107] Comparative Example 6
[0108] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0109] The other conditions are consistent with those in Example 3, except that the final temperature of the heat treatment in step (3) is 1150° C. The main crystal phase of the obtained fiber is t-ZrO2, with only a small amount of θ-Al2O3; it can be seen that the change of the heat treatment temperature will affect the formation of the crystal phase in the fiber.
[0110] Comparative Example 7
[0111] A method for preparing zirconium oxide-aluminum oxide composite short fibers comprises the following steps:
[0112] The other conditions were the same as those in Example 3, except that the precursor fiber prepared in step (2) was placed in a muffle furnace, heated at a rate of 8°C / min until it reached 1300°C, and kept at this temperature for 1 hour. The prepared fiber was severely powdered. It can be seen that a too fast heating rate is not conducive to the heat treatment of the fiber.
[0113] The experimental processes of Examples 1-6 and Comparative Examples 1-7 were observed and the diameter and length of the obtained fibers were tested. The results are shown in the following figure.
[0114] Table 1 Experimental phenomena or test results of fiber diameter and length obtained in Examples 1-6 and Comparative Examples 1-7
[0115]
[0116]
[0117] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing an aluminum-zirconium composite spinning solution, It is characterized in that The aluminum-zirconium composite spinning solution is prepared by a sol-gel method using aluminum hydroxide, zirconium hydroxide, organic carboxylic acid, yttrium acetate and boric acid as raw materials; After mixing organic carboxylic acid and water, aluminum hydroxide is added, and condensation reflux is performed at 70-95° C. for 8-10 hours, and then zirconium hydroxide is added, and condensation reflux is continued for 10-30 minutes; carboxylic acid aluminum zirconium sol is obtained by cooling and filtering, and yttrium acetate, boric acid and polyvinyl alcohol are added to the carboxylic acid aluminum zirconium sol, and aluminum zirconium composite spinning solution is obtained by vacuum distillation; The molar ratio of aluminum hydroxide to organic carboxylic acid is 1:1-2.5; the molar ratio of aluminum hydroxide to water is 1:10-20; the molar ratio of aluminum hydroxide to zirconium hydroxide is 10-25:1; the molar ratio of zirconium hydroxide to yttrium acetate is 15-50:1; and the molar ratio of aluminum hydroxide to boric acid is 28-108:
1.
2. The method for preparing the aluminum-zirconium composite spinning solution according to claim 1, It is characterized in that The amount of polyvinyl alcohol added is 0.2-1.4wt% of the total mass of the raw materials.
3. The method for preparing the aluminum-zirconium composite spinning solution according to claim 1, It is characterized in that The organic carboxylic acid is one or more of formic acid, acetic acid, oxalic acid, malonic acid and citric acid.
4. The method for preparing the aluminum-zirconium composite spinning solution according to claim 1, It is characterized in that The temperature of the reduced pressure distillation is 40-50°C, and the distillation is performed to a viscosity of 300-800 Pa·s.
5. A method for preparing a precursor fiber, It is characterized in that The aluminum-zirconium composite spinning solution prepared by any one of claims 1 to 4 is subjected to vacuum degassing, and then the spinning solution is spun under the conditions of an ambient temperature of 20-30° C. and a relative humidity of 15-35%, and the precursor fiber is obtained after drawing, dropping and short cutting.
6. The method for preparing the precursor fiber according to claim 5, It is characterized in that The spinning solution is spun using a metering pump, and the flow rate of the metering pump is 30-60cc / min.
7. A method for preparing zirconium oxide-aluminum oxide composite short fibers, It is characterized in that The precursor fiber prepared as claimed in any one of claims 5 to 6 is placed in a muffle furnace, first slowly heated to 100-150°C, and then kept at this temperature for 0.5-1h; then slowly heated to 600-700°C, and kept at this temperature for 0.5-1h; finally heated to 1200-1400°C, and kept at this temperature for 0.5-2h to obtain zirconia-alumina composite short fibers.
8. The method for preparing the zirconium oxide-aluminum oxide composite short fibers according to claim 7, It is characterized in that The temperature is increased to 100-150°C at a rate of 0.1-1.0°C / min, the temperature is increased to 600-700°C at a rate of 0.5-3.0°C / min, and the temperature is increased to 1200-1400°C at a rate of 5-10°C / min.