A nanofiber composite film and preparation method thereof, and a friction nanogenerator
BaTiO3:La nanoparticles are combined with PVDF-TrFE through an electrospinning process to prepare a nanofiber composite film, which solves the problem of low output performance of triboelectric nanogenerators, achieves efficient power conversion and wireless energy transmission, and is suitable for a variety of media , promoting the development of power supply for portable electronic devices.
Patent Information
- Application Number
- CN202211633871.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-19
AI Technical Summary
The low output performance of triboelectric nanogenerators limits their wide application in power supply for portable electronic devices, and existing improvement methods require complex processes and equipment, hindering large-scale production.
The electrospinning process was used to combine the BaTiO3:La nanoparticles prepared by the hydrothermal method with PVDF-TrFE to prepare a nanofiber composite film to improve the output performance of the triboelectric nanogenerator.
The open-circuit voltage, short-circuit current density, transferred charge density and power density of the triboelectric nanogenerator are significantly improved, achieving low-cost, high-efficiency power conversion, suitable for a variety of transmission media, and supporting wireless energy transmission.
Smart Images

Figure CN115897069B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nanometer power generation materials, and in particular relates to a nanometer fiber composite film and a preparation method thereof, and a friction nanometer generator. Background Art
[0002] With the rapid development of artificial intelligence and the Internet of Things, the demand for portable electronic devices has exploded, which has put forward higher requirements for the device power supply system. Due to the huge number and widespread distribution of small electronic products, it is difficult to meet the energy demand by using traditional battery devices alone, and it is not conducive to the miniaturization of devices. In recent years, people have paid attention to the collection of biomechanical energy from the surrounding environment to power these electronic systems.
[0003] As a new type of green energy device, the friction nanogenerator can convert the ubiquitous but wasted mechanical energy in the environment into electrical energy through the coupling of frictional charging and electrostatic induction. It has broad application prospects in wearable electronic devices, the Internet of Things, the environment, and medical fields, and also provides an effective strategy for the power supply problem of electronic devices. However, the friction nanogenerator generally has the problem of low output performance, which restricts the wider practical application of the friction nanogenerator.
[0004] Material surface patterning, material surface chemical modification, and charge injection are conventional methods used in the prior art to improve the output performance of triboelectric nanogenerators. However, the above methods often require matching complex processes, special equipment, or complex device structures, which seriously hinders the large-scale production of triboelectric nanogenerators.
[0005] Therefore, designing and developing a new type of friction material with low cost, high efficiency, excellent output performance and cycle stability to enhance the output performance of friction nanogenerators is of great significance in solving the power supply problem of portable electronic devices. Summary of the invention
[0006] In order to solve the above problems, the first purpose of the present invention is to provide a method for preparing a nanofiber composite film. When the nanofiber composite film prepared by this method is used as a friction material of a friction nanogenerator, the output performance of the friction nanogenerator can be greatly improved.
[0007] The second object of the present invention is to provide a nanofiber composite film, which can greatly improve the output performance of the friction nanogenerator and is suitable for use in the friction nanogenerator.
[0008] The third object of the present invention is to provide a friction nanogenerator having excellent output performance.
[0009] A fourth objective of the present invention is to provide a method for wireless energy transmission, which is applicable to a variety of transmission media.
[0010] The fifth purpose of the present invention is to provide a biomechanical energy collection and wireless energy transmission system, which uses a friction nanogenerator to convert biomechanical energy into electrical energy and transmits wireless energy. After the voltage signal is processed by the circuit, it can trigger the operation of electronic equipment in real time.
[0011] The method for preparing the nanofiber composite film of the present invention adopts the following technical scheme:
[0012] A method for preparing a nanofiber composite film comprises the following steps:
[0013] (1) mixing BaTiO3:La nanoparticles with a solvent to obtain a suspension; then adding PVDF-TrFE powder to the suspension to obtain an electrospinning precursor solution; the BaTiO3:La nanoparticles are La-doped BaTiO3 nanoparticles prepared by a hydrothermal method; the molar percentage content of La in the BaTiO3:La nanoparticles is 0.6-0.8%;
[0014] (2) Electrospinning the electrospinning precursor solution to obtain a nanofiber composite film.
[0015] The method for preparing the nanofiber composite film of the present invention combines the friction material matrix PVDF-TrFE with BaTiO3:La nanoparticles through an electrospinning process to prepare the nanofiber composite film. The present invention has found and confirmed through research experiments that by successfully introducing BaTiO3:La nanoparticles prepared by a hydrothermal method into PVDF-TrFE, the dielectric constant of the composite film can be effectively improved, and after being applied to the friction nanogenerator, the output performance of the friction nanogenerator can be greatly improved.
[0016] In addition, the BaTiO3:La nanoparticles used in the present invention are synthesized by a hydrothermal method. The BaTiO3:La nanoparticles synthesized by a hydrothermal method can not only provide a new material option for improving the output performance of tribo-nanoelectric power generation, but also expand the application scope and application value of the BaTiO3:La nanoparticles.
[0017] The present invention uses experiments to verify that the BaTiO3:La nanoparticles prepared by the hydrothermal method have better microscopic morphology and doping effect, which is beneficial to the improvement of the output performance of the friction generator. Preferably, the preparation process of the BaTiO3:La nanoparticles includes the following steps:
[0018] (a) dissolving tetrabutyl titanate in anhydrous ethanol, and then adding ammonia water to obtain solution A;
[0019] Separately, dissolve barium hydroxide and lanthanum nitrate in water to obtain solution B;
[0020] (b) transferring solution B into solution A, adding diethanolamine and stirring to obtain a suspension;
[0021] (c) placing the suspension in a hydrothermal reactor for hydrothermal reaction at 190-210° C. for 40-50 h to obtain BaTiO 3 :La nanoparticles.
[0022] Preferably, the barium hydroxide is barium hydroxide monohydrate; the lanthanum nitrate is lanthanum nitrate hexahydrate; and after the hydrothermal reaction, the method further includes the steps of centrifuging, washing and drying the reaction product.
[0023] The present invention adopts the above-mentioned hydrothermal reaction process, the operation steps are simple and easy, the raw material price is extremely low, and it is easy to mass produce. In order to control the microscopic morphology and synthesis quality of BaTiO3:La nanoparticles, the output performance of the nano friction generator is further improved. Preferably, in solution A, the dosage ratio of tetrabutyl titanate, anhydrous ethanol, and ammonia water is 8.509g:10mL:3.5mL. In solution B, the dosage ratio of monohydrated barium hydroxide, hexahydrated lanthanum nitrate, and water is 7.102g:0.1227g:12mL. The dosage of diethanolamine is 2.5mL. Further preferably, the conditions of the hydrothermal reaction are: 200℃ hydrothermal reaction for 48h. The molar percentage content of La in the prepared BaTiO3:La nanoparticles is 0.7%. The present invention adopts the above method to prepare the obtained BaTiO3:La nanoparticles, which have a consistent morphology, are uniformly cubic, and have an average particle size of 80-120nm, which is very suitable for incorporation into PVDF-TrFE nanofibers. Moreover, experiments have confirmed that the use of BaTiO3:La nanoparticles can enhance the ability of the composite film to store charge by increasing the dielectric constant of the composite film, thereby improving the output performance of the friction nanogenerator.
[0024] Preferably, in step (1), the solvent is N,N-dimethylformamide (DMF).
[0025] Furthermore, in step (1), the specific process of preparing the suspension is: adding BaTiO3:La nanoparticles to the solvent, first stirring at a speed of 400-600 rpm for 100-150 min, and then ultrasonically vibrating at a power of 90-120 W for 10-20 min; the specific process of preparing the electrospinning precursor solution is: adding PVDF-TrFE powder to the suspension, first ultrasonically vibrating at a power of 60-80 W for 100-150 min, and then stirring at a speed of 400-600 rpm for 50-70 min.
[0026] More preferably, the sonication is performed using an ultrasonic cell disruptor.
[0027] In the present invention, PVDF-TrFE powder is used as the friction material matrix when preparing the electrospinning precursor solution. PVDF-TrFE is polyvinylidene chloride-trifluoroethylene, which is a high molecular polymer. Preferably, in the PVDF-TrFE powder, the molecular weight of PVDF-TrFE is 100,000 to 120,000.
[0028] As a further preferred solution, in step (1), the mass concentration of PVDF-TrFE powder in the electrospinning precursor solution is 28-32wt.%, more preferably 30wt.%. The mass ratio of BaTiO3:La nanoparticles to PVDF-TrFE powder is (0.015-0.020):(3.4-3.6), more preferably 0.0175:3.5.
[0029] Preferably, in step (2), the electrospinning conditions are: the spinning voltage is 12kV to 14kV, and the spinning time is 40 to 50min. More preferably, the spinning voltage is 13kV, and the spinning time is 45min. Further, the propulsion rate of the electrospinning precursor solution is 3mL / h, the collector collection rate is 500rpm, and the receiving distance between the syringe tip and the collector is 15cm.
[0030] In step (2), the diameter of a single fiber in the obtained nanofiber composite film is 500 to 1000 nm.
[0031] The nanofiber composite film of the present invention adopts the following technical solution:
[0032] A nanofiber composite film is prepared by the above-mentioned method for preparing the nanofiber composite film.
[0033] The nanofiber composite film of the present invention can improve the dielectric constant of PVDF-TrFE and increase the difference in the ability of the friction material to gain and lose electrons by successfully introducing BaTiO3:La nanoparticles into PVDF-TrFE, thereby achieving a significant improvement in the output performance of the friction nanogenerator.
[0034] The friction nanogenerator of the present invention adopts the following technical solution:
[0035] A friction nanogenerator comprises a positive friction material and a negative friction material; the negative friction material comprises a substrate and the nanofiber composite film as described above.
[0036] Further preferably, the positive friction material is a nitrile film; and the substrate is an aluminum foil.
[0037] The friction nanogenerator of the present invention uses a nanofiber composite film as a negative friction material. The present invention has confirmed through electrical performance test that the open circuit voltage, short circuit current density, transfer charge density, and power density of the friction nanogenerator based on the composite film have been greatly improved, giving the friction nanogenerator excellent output performance. In addition, the friction nanogenerator of the present invention is also non-toxic and tasteless, small in size, and light in weight, and has important value for the development of high-performance micro-nano devices.
[0038] The method for wireless energy transmission of the present invention adopts the following technical solution:
[0039] A method for wireless energy transmission, wherein the wireless energy transmission is performed using the friction nanogenerator, antenna and signal acquisition device as described above; the signal acquisition device includes an oscilloscope and an electrometer.
[0040] Preferably, the antenna consists of only a receiving end antenna; or the antenna consists of a transmitting end antenna and a receiving end antenna.
[0041] Furthermore, in the method for wireless energy transmission, the transmission medium used includes air and liquid medium; the liquid medium includes but is not limited to pure water, sea water, alcohol, and serum.
[0042] The wireless energy transmission method of the present invention, the voltage and current signals of the friction nanogenerator can be used for wireless energy transmission in media including air, household drinking water and high-concentration salt water, etc. It can be transmitted in different media such as air and water without any transmitting device, has a wide range of applications, and the transmission process is simple and the electrical signal is high.
[0043] The biomechanical energy collection and wireless energy transmission system of the present invention adopts the following technical solutions:
[0044] A biomechanical energy collection and wireless energy transmission system comprises the friction nanogenerator, a wireless control module and an electronic device as described above.
[0045] Preferably, the wireless control module includes a signal receiving antenna, a circuit processing module and a Bluetooth module. Further, the circuit processing module includes an amplification circuit and an analog-to-digital conversion circuit. The electronic device includes a common low-power electronic device such as a toy car and a pedometer.
[0046] In the biomechanical energy collection and wireless energy transmission system constructed by the present invention, the friction nanogenerator can directly collect low-frequency biomechanical energy in the environment and convert it into electrical energy, and its voltage and current signals can be transmitted in different media such as air and water without any transmitting device. In particular, the voltage signal can be wirelessly transmitted 3.5 meters in the air and captured by the antenna, and then can trigger low-power electronic devices to work in real time after circuit processing. It has broad application prospects in energy collection and wireless transmission, such as implantable medical devices, encrypted wireless communications, smart home appliances and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is a microscopic morphology of BaTiO3:La nanoparticles prepared in Example 1 of the present invention;
[0048] Figure 2 This is a particle size distribution diagram of BaTiO3:La nanoparticles prepared in Example 1 of the present invention;
[0049] Figure 3 This is a microscopic morphology of the BaTiO3:La / PVDF-TrFE nanofiber composite film prepared in Example 1 of the present invention;
[0050] Figure 4 This is a diagram of the internal structure of a single BaTiO3:La / PVDF-TrFE nanofiber prepared in Example 1 of the present invention;
[0051] Figure 5 The open circuit voltage diagram of the friction nanogenerator of Example 2 of the present invention and Comparative Example 1 at an impact frequency of 1.5 Hz;
[0052] Figure 6 It is a short-circuit current density diagram of the friction nanogenerator of Example 2 of the present invention and Comparative Example 1 at an impact frequency of 1.5 Hz;
[0053] Figure 7 The transferred charge density diagram of the friction nanogenerator of Example 2 of the present invention and Comparative Example 1 at an impact frequency of 1.5 Hz;
[0054] Figure 8 The output power density diagram of the nanogenerators of Example 2 of the present invention and Comparative Example 1 at an impact frequency of 1.5 Hz;
[0055] Fig. 9 The dielectric constant diagram of the nanofiber composite film of Example 1 of the present invention and Comparative Example 1, the horizontal axis is the frequency of the electric field applied during the test;
[0056] Fig.10 It is a schematic diagram of the wireless energy transmission method according to Embodiment 3 of the present invention transmitted in the air;
[0057] Fig.11 This is a diagram of wireless voltage signals after wireless energy transmission in the air in Example 3 of the present invention;
[0058] Fig.12 This is a radio current signal diagram after wireless energy transmission in the air in Example 3 of the present invention;
[0059] Fig.13 is a relationship diagram of wireless voltage and current signals in the air as the transmission distance changes in Example 3 of the present invention;
[0060] Fig.14 This is a physical picture of lighting a commercial LED lamp through wireless energy transmission in Example 3 of the present invention;
[0061] Fig.15 It is a schematic diagram of the wireless energy transmission method according to Embodiment 3 of the present invention in air and liquid medium;
[0062] Fig.16 This is a diagram of wireless voltage signals after wireless energy transmission in air and different liquid media in Example 3 of the present invention;
[0063] Fig.17 This is a radio current signal diagram after wireless energy transmission in air and different liquid media in Example 3 of the present invention;
[0064] Fig.18 Schematic diagram of wireless energy transmission in different liquid media according to the wireless energy transmission method of embodiment 3 of the present invention;
[0065] Fig.19 This is a diagram of wireless voltage signals after wireless energy transmission in different liquid media in Example 3 of the present invention;
[0066] Fig. 20 A radio current signal diagram after wireless energy transmission in different liquid media in Example 3 of the present invention;
[0067] Fig.21 It is a schematic diagram of the biomechanical energy collection and wireless energy transmission system in Example 4 of the present invention;
[0068] Fig. 22 is a circuit schematic diagram of the circuit processing module in Embodiment 4 of the present invention;
[0069] Fig.23 A physical picture of triggering the operation of a toy car based on the biomechanical energy collection and wireless energy transmission system in Example 4 of the present invention;
[0070] Fig.24 This is a physical picture of triggering the operation of a pedometer based on the biomechanical energy collection and wireless energy transmission system in Example 4 of the present invention. DETAILED DESCRIPTION
[0071] The technical scheme of the present invention is further described below in conjunction with specific embodiments, but does not constitute a limitation of the present invention. The specific conditions not described in the following examples are all carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or raw materials used in the following examples, unless otherwise specified, are conventional products obtained through commercial channels.
[0072] Among them, the PVDF-TrFE powder used in the following examples has VDF / TrFE=85 / 15 mol and a molecular weight of 110000, which was purchased from Dongguan Zhanyang Polymer Materials Co., Ltd., and the manufacturer is Arkema of France, model 2801-01. The manufacturer of the electrospinning equipment used in the following examples is Dongwen High Voltage Power Supply (Tianjin) Co., Ltd., and the model is JDF05 electrospinning machine.
[0073] Example 1
[0074] This embodiment provides a method for preparing a nanofiber composite film and an embodiment of the nanofiber composite film.
[0075] Before preparing the nanofiber composite film, the hydrothermal preparation of BaTiO3:La nanoparticles is first performed, and the specific steps are as follows:
[0076] (a) 8.509 g of tetrabutyl titanate was added to 10 mL of anhydrous ethanol, and the mixture was stirred for 20 min. Then, 3.5 mL of aqueous ammonia was added to obtain solution A. 7.102 g of barium hydroxide monohydrate and 0.1227 g of lanthanum nitrate hexahydrate were added to 12 mL of deionized water at 90° C., and the mixture was stirred for 20 min to obtain solution B.
[0077] (b) Pour solution B completely into solution A and add 2.5 mL of diethanolamine and stir for 10 min to form a suspension.
[0078] (c) The obtained suspension was sealed in a 100 mL Teflon autoclave and subjected to hydrothermal reaction at 200° C. for 48 h. After the reaction, the solution was centrifuged, the upper clear liquid was discarded, the lower white solid particles were washed with ethanol and deionized water several times, and finally dried in a vacuum drying oven at 80° C. for 48 h to obtain BaTiO3:La nanoparticles. The molar percentage content of La in the BaTiO3:La nanoparticles was 0.7%.
[0079] The method for preparing the nanofiber composite film of this embodiment comprises the following steps:
[0080] (1) 0.0175 g of the BaTiO3:La nanoparticles prepared by the above method was added to 8 g of DMF solution, stirred at 500 rpm for 2 h, and then an ultrasonic cell crusher was used to excite the BaTiO3:La nanoparticles to vibrate for 15 min at a power of 100 W to make them evenly distributed, thereby obtaining a suspension;
[0081] 3.5 g of PVDF-TrFE powder was added to the above suspension, and ultrasonic vibration was performed for 2 h at 70 W using an ultrasonic cell crusher, and then stirred at 500 rpm for 1 h to obtain a uniform milky white electrospinning precursor solution with a mass concentration ratio of 30 wt.%.
[0082] (2) The electrospinning precursor solution obtained in step (1) was loaded into a 10 mL syringe, which was then installed on the propulsion pump of the electrospinning equipment. The propulsion rate was set to 3 mL / h, the collector collection rate was 500 rpm, the receiving distance was 15 cm, the spinning high voltage source was 13 kV, and aluminum foil was placed on the receiver. The prepared solution was electrospun onto the surface of the aluminum foil substrate for 45 min to obtain a PVDF-TrFE nanofiber composite film with BaTiO3:La nanoparticles added. Finally, the obtained nanofiber composite film was placed in a 60°C drying oven and dried at a constant temperature for 1 h to allow the solvent to fully evaporate, thereby obtaining the nanofiber composite film of Example 1 (denoted as BaTiO3:La / PVDF-TrFE).
[0083] Example 2
[0084] This embodiment is an embodiment of a friction nanogenerator.
[0085] The friction nanogenerator of this embodiment includes a positive friction material and a negative friction material; the negative friction material includes a substrate and the nanofiber composite film of embodiment 1. The positive friction material is a nitrile film; and the substrate is an aluminum foil.
[0086] The specific preparation method of the friction nanogenerator of this embodiment is as follows: the nanofiber composite film of Example 1 is cut into 3×3 cm 2 A small-sized film is made, and then aluminum foil is used as the film substrate, the substrate aluminum foil is used as an electrode and connected to a copper wire to draw out the current, thereby obtaining the negative friction material of the friction nanogenerator; a nitrile film of the same size is cut from a nitrile glove as the positive friction material of the friction nanogenerator, thus forming a single-electrode mode friction nanogenerator.
[0087] In other embodiments, the friction nanogenerator, in addition to the single-electrode mode friction nanogenerator, can also be any one of a vertical contact-separation friction nanogenerator, a horizontal sliding friction nanogenerator, and an independent layer friction nanogenerator.
[0088] Example 3
[0089] This embodiment is a method embodiment of wireless energy transmission.
[0090] The wireless energy transmission method provided in this embodiment is performed using the friction nanogenerator, receiving end antenna and signal acquisition device of embodiment 2. The signal acquisition device includes an oscilloscope and an electrometer. In this embodiment, the receiving end antenna is a 5×5 cm 2 Aluminum foil is used to place the receiving antenna in the air medium, and the antenna is connected to the signal collection device through a metal wire. The friction nanogenerator is triggered by clapping, and the energy generated is wirelessly transmitted in the air and received by the antenna at a certain distance. The voltage signal after wireless energy transmission can be collected by an oscilloscope, and the current signal can be collected by an electrometer. The electrometer uses a Keithley 6514 high-resistance electrometer.
[0091] In other embodiments, the method of wireless energy transmission is performed using the friction nanogenerator, the transmitting end antenna, the receiving end antenna and the signal acquisition device of Example 2. The friction nanogenerator is the single-electrode mode friction nanogenerator prepared in Example 2. The transmitting end antenna is a 5×5 cm 2 The aluminum foil is encapsulated with polyimide tape and connected to the aluminum foil electrode of the friction nanogenerator through a metal wire; the signal end antenna is a 5×5cm 2 The aluminum foil is wrapped with polyimide tape, and then the signal end antenna is placed in the liquid medium; the signal acquisition device includes an oscilloscope and an electrometer, and the receiving end antenna is connected to the acquisition device through a metal wire. The friction nanogenerator is triggered by clapping, and the energy generated is emitted from the transmitting end antenna, which can be wirelessly transmitted in different media such as air and liquid, and received by the antenna at a certain distance. The transmitted wireless voltage signal can be collected by the oscilloscope, and the wireless current signal can be collected by the electrometer. The liquid media used include household drinking water and high-concentration salt water.
[0092] In other embodiments, the method of wireless energy transmission is performed using the friction nanogenerator, the transmitting end antenna, the receiving end antenna and the signal acquisition device of Example 2. The friction nanogenerator is the single-electrode mode friction nanogenerator prepared in Example 2. The transmitting end antenna is a 5×5 cm 2 The aluminum foil is encapsulated with polyimide tape and connected to the aluminum foil electrode of the friction nanogenerator through a metal wire; the signal end antenna is a 5×5cm 2The aluminum foil is wrapped with polyimide tape, and then the transmitting antenna and the receiving antenna are placed in the liquid medium; the signal acquisition device includes an oscilloscope and an electrometer, and the receiving antenna and the acquisition device are connected by metal wires. The friction nanogenerator is triggered by clapping, and the energy generated is emitted from the transmitting antenna, which can be transmitted in different liquid media and sensed by the receiving antenna at a certain distance. The transmitted wireless voltage signal can be collected by the oscilloscope, and the wireless current signal can be collected by the electrometer. The liquid media used include household drinking water and high-concentration salt water.
[0093] In other embodiments, the antenna may also be made of conductive metals such as iron, nickel, gold, aluminum alloy, copper alloy, iron alloy, silver alloy, etc. The antenna may also be improved by using different shapes, which will not be described in detail. In addition, in different embodiments, the liquid medium may also be pure water, seawater, alcohol, serum, etc., which is not specifically limited in the present invention.
[0094] Example 4
[0095] This embodiment is an embodiment of a biomechanical energy collection and wireless energy transmission system. The biomechanical energy collection and wireless energy transmission system provided in this embodiment includes the friction nanogenerator, wireless control module and electronic device of Example 2. The friction nanogenerator is triggered by clapping to collect biomechanical energy and convert it into electrical energy, as well as transmit voltage signals. The wireless control module includes a signal receiving antenna, a circuit processing module, a Bluetooth module and a single-chip microcomputer. The signal receiving antenna is a 10×5 cm 2 Aluminum foil is connected to the signal input end of the circuit processing module, and the circuit processing module includes an amplifier circuit AD620 and an analog-to-digital conversion circuit LM393N; the voltage signal can be received and processed by the wireless control module. When the Bluetooth module in the wireless control module receives the digital signal processed by the circuit processing module, the Arduino uno microcontroller analyzes and processes the digital signal according to the program code, and then sends the corresponding digital signal to the electronic device to make it work. In different embodiments, the electronic device can be a common low-power electronic device such as a toy car and a pedometer.
[0096] Test example
[0097] Experimental Example 1 Structural Characterization of BaTiO3:La Nanoparticles
[0098] The SEM (scanning electron microscope) microscopic morphology of the BaTiO3:La nanoparticles prepared in Example 1 is as follows Figure 1 The particle size distribution is shown in Figure 2 shown.
[0099] Depend on Figure 1It can be seen that the BaTiO3:La nanoparticles have consistent morphology and are in a uniform cubic shape.
[0100] Depend on Figure 2 It can be seen that the particle size of BaTiO3:La nanoparticles is small, with an average size of 80-120 nm, which is conducive to its successful incorporation into PVDF-TrFE nanofibers.
[0101] Experimental Example 2 Structural Characterization of Nanofiber Composite Film
[0102] The SEM microscopic morphology of the nanofiber composite film of Example 1 is as follows: Figure 3 As shown. Figure 3 It can be seen that the nanofiber composite film of Example 1 has an obvious fiber structure inside, and the diameter of a single fiber is 500-1000 nm.
[0103] The TEM (transmission electron microscope) internal structure of a single BaTiO3:La / PVDF-TrFE nanofiber in the nanofiber composite film is shown in Figure 1. Figure 4 As shown. Figure 4 It can be seen that BaTiO3:La nanoparticles are embedded in the PVDF-TrFE nanofibers.
[0104] Experimental Example 3 Output performance of friction nanogenerator and dielectric constant test of nanofiber composite film
[0105] A pure PVDF-TrFE nanofiber film without nanoparticles was used as comparative example 1 to prepare a friction nanogenerator of the same specification as that of Example 2. The friction nanogenerator based on the pure PVDF-TrFE nanofiber film of comparative example 1 and the friction nanogenerator based on the BaTiO3:La / PVDF-TrFE nanofiber composite film of Example 2 were tested for electrical properties of open circuit voltage, short circuit current density, transfer charge density, and output power density at an impact frequency of 1.5 Hz. At the same time, the dielectric constant of the pure PVDF-TrFE nanofiber film of comparative example 1 and the BaTiO3:La / PVDF-TrFE nanofiber composite film of Example 1 were tested.
[0106] The electrical performance process is as follows: use a conductive copper wire to connect the base aluminum foil of the BaTiO3:La / PVDF-TrFE nanofiber composite film to the positive electrode interface of the Keithley 6514 high resistance electrometer, and ground the ground terminal and the negative electrode of the electrometer. Adjust the corresponding gear and sensitivity of the electrometer to achieve accurate measurement of low current, high resistance source voltage and charge. The signal collected by the NI data acquisition card 152805A can be displayed in real time on the corresponding computer screen. The dielectric constant test process is as follows: First, cut the BaTiO3:La / PVDF-TrFE nanofiber composite film into 2×2cm 2 The area of the film was measured and the aluminum foil at the bottom was removed. A manual coater was used to apply silver paste of uniform thickness on both sides of the film as upper and lower electrodes. The prepared sample was placed on the probe station of an impedance analyzer (Agilent model 4294A). The capacitance was obtained by changing the operating frequency, and the dielectric constant was obtained by conversion using the formula.
[0107] The test results of the electrical output performance of the friction nanogenerators of Example 2 and Comparative Example 1 are as follows: Figures 5 to 8 The dielectric constants of the pure PVDF-TrFE nanofiber film of Comparative Example 1 and the BaTiO3:La / PVDF-TrFE nanofiber composite film of Example 1 are shown in Fig. 9 As shown. Among them, Figure 5 Graph showing the open circuit voltage of the friction nanogenerators of Example 2 and Comparative Example 1 at an impact frequency of 1.5 Hz. Figure 6 Graph showing the short-circuit current density of the friction nanogenerators of Example 2 and Comparative Example 1 at an impact frequency of 1.5 Hz. Figure 7 Graph showing the charge transfer density of the friction nanogenerators of Example 2 and Comparative Example 1 at an impact frequency of 1.5 Hz. Figure 8 The output power density diagram of the friction nanogenerator of Example 2 and Comparative Example 1 at an impact frequency of 1.5 Hz.
[0108] Combination Figures 5 to 8 The test results show that the open circuit voltage, short circuit current density, transfer charge density and power density of the friction nanogenerator based on BaTiO3:La / PVDF-TrFE nanofiber composite film in Example 2 of the present invention reached 245V, 19.2mA / m 2 、87.3μC / m 2 , 2.52W / m 2 , which are 3, 4, 3, and 11 times of the triboelectric nanogenerator based on pure PVDF-TrFE nanofiber film in comparative example 1. This test result directly confirms that the output performance of the triboelectric nanogenerator can be greatly enhanced by adding BaTiO3:La nanoparticles to PVDF-TrFE to form a composite film.
[0109] Depend on Fig. 9 It can be seen that at a frequency of 10kHz, the dielectric constant of the pure PVDF-TrFE nanofiber film of Comparative Example 1 is 12.0, while the dielectric constant of the BaTiO3:La / PVDF-TrFE nanofiber composite film of Example 1 reaches 38.8, which confirms that the present invention adds BaTiO3:La nanoparticles to PVDF-TrFE to construct a composite film, which can significantly improve the dielectric constant of the composite film. It can be seen that the nanofiber composite film provided by the present invention uses electrospinning technology to embed BaTiO3:La nanoparticles in PVDF-TrFE nanofibers, which can effectively improve the dielectric constant of the composite film and significantly improve the ability of the composite film to store charge, thereby enhancing the output performance of the friction nanogenerator.
[0110] Test Example 4 Electrical signal test of wireless energy transmission method
[0111] The schematic diagram of the wireless energy transmission method of Example 3 in the air medium is as follows: Fig.10 After the energy generated by the wireless energy transmission method of Example 3 is wirelessly transmitted in the air, the collected wireless voltage and current signals are respectively as shown in Fig.11 and Fig.12 When wireless voltage and current signals are transmitted in the air, they will attenuate as the distance increases, as shown in Figure 2. Fig.13 As shown. Fig.13 It can be seen that the effective distance of voltage transmission can reach 3.5 meters, and the effective distance of current transmission can reach 35 centimeters. The actual picture of lighting up LED lights using wireless energy transmission characteristics is as follows Fig.14 As shown. Fig.14 It can be seen that commercial LED lights can be wirelessly lit up by simply clapping your hands to trigger the friction nanogenerator without any additional energy transmission device.
[0112] The schematic diagram of the wireless energy transmission method of Example 3 in air and liquid medium is as follows: Fig.15 The wireless voltage signal and current signal after wireless energy transmission in air and different liquid media are shown in Figure 1. Fig.16 and Fig.17 As shown. Fig.16 , 17 It can be seen that the electrical signal received after transmission in high-concentration salt water is higher than that in household drinking water.
[0113] The schematic diagram of the wireless energy transmission method of Example 3 in different liquid media is as follows: Fig.18 The wireless voltage signal and current signal after wireless energy transmission in different liquid media are shown in Figure 1. Fig.19 and Fig. 20 As shown. Fig.19 ,20 It can be seen that the electrical signal received after transmission in high-concentration salt water is higher than that in household drinking water.
[0114] Experimental Example 5 Specific application of biomechanical energy harvesting and wireless energy transmission system
[0115] The schematic diagram of the biomechanical energy collection and wireless energy transmission system of Example 4 of the present invention is shown in FIG. Fig.21 As shown in the figure, by tapping the friction nanogenerator with your hand, you can achieve long-distance wireless triggering of electronic devices. The circuit diagram of the circuit processing module is shown in the figure. Fig. 22 The actual pictures of triggering the toy car and pedometer based on the biomechanical energy collection and wireless energy transmission system are shown in Figure 1. Fig.23 and Fig.24 shown.
[0116] In summary, the present invention adopts electrostatic spinning to incorporate BaTiO3:La nanoparticles into PVDF-TrFE to prepare a nanofiber composite film, and the open circuit voltage, short circuit current density, transfer charge density, and power density of the friction nanogenerator based on the composite film are greatly improved. At the same time, the present invention provides a wireless energy transmission method based on the friction nanogenerator, which can realize energy transmission in a variety of media by clapping the friction nanogenerator, and its wireless voltage and wireless current signals can be collected in real time. In addition, the present invention constructs a biomechanical energy collection and wireless energy transmission system based on the high-performance friction nanogenerator, which uses the friction nanogenerator to collect and convert low-frequency biomechanical energy in the environment into electrical energy, and its voltage signal can be wirelessly transmitted to the antenna end, and after being processed by the wireless control circuit, it triggers the low-power electronic device to work in real time, showing good promotion and application potential in the fields of implantable medical devices, encrypted wireless communications, smart home appliances, etc.
Claims
1. A method for preparing a nanofiber composite film, characterized in that: The following steps are involved: (1) Tetrabutyl titanate is dissolved in anhydrous ethanol, and then ammonia water is added to obtain solution A; barium hydroxide and lanthanum nitrate are dissolved in water to obtain solution B; solution B is transferred to solution A, diethanolamine is added and stirred to obtain a suspension; the suspension is subjected to a hydrothermal reaction in a hydrothermal reactor at 190-210° C. for 40-50 hours to obtain BaTiO3:La nanoparticles; (2) mixing BaTiO3:La nanoparticles with a solvent to obtain a suspension; then adding PVDF-TrFE powder to the suspension to obtain an electrospinning precursor solution; the BaTiO3:La nanoparticles are La-doped BaTiO3 nanoparticles prepared by a hydrothermal method; the molar percentage content of La in the BaTiO3:La nanoparticles is 0.6-0.8%; (3) electrospinning the electrospinning precursor solution to obtain a nanofiber composite film; Wherein, the preparation process of the suspension in step (2) is specifically as follows: BaTiO3:La nanoparticles are added to the solvent, first stirred at a speed of 400-600rpm for 100-150min, and then ultrasonically vibrated for 10-20min at a power of 90-120W; the solvent is one of N,N-dimethylformamide, dimethyl sulfoxide, and dimethyl ketone; the preparation process of the electrospinning precursor solution is specifically as follows: PVDF-TrFE powder is added to the suspension, first ultrasonically vibrated for 100-150min at a power of 60-80W, and then stirred at a speed of 400-600rpm for 50-70min; in the electrospinning precursor solution, the mass concentration of PVDF-TrFE powder is 28-32wt.%; the mass ratio of BaTiO3:La nanoparticles to PVDF-TrFE powder is (0.015-0.020): (3.4-3.6).
2. The method for preparing the nanofiber composite film according to claim 1, characterized in that: In step (3), the conditions for the electrospinning are: the spinning voltage is 12 kV to 14 kV, and the spinning time is 40 to 50 min.
3. A nanofiber composite film, characterized in that: The nanofiber composite film is prepared by the method for preparing the nanofiber composite film according to claim 1.
4. A friction nanogenerator, characterized in that: It comprises a positive friction material and a negative friction material; the negative friction material comprises a substrate and the nanofiber composite film according to claim 3.
5. A method for wireless energy transmission, characterized in that: The wireless energy transmission is performed using the friction nanogenerator, antenna and signal acquisition device described in claim 4; the signal acquisition device includes an oscilloscope and an electrometer.
6. A biomechanical energy collection and wireless energy transmission system, characterized in that: It comprises the friction nanogenerator as claimed in claim 4, a wireless control module and an electronic device.
Citation Information
Patent Citations
Multifunctional piezoelectric nanofiber material, flexible sensor and preparation method of multifunctional piezoelectric nanofiber material and preparation method of flexible sensor
CN112899806A