A preparation method of silicon oxide composite material and its product and application in lithium ion battery

By blending the fine powder of silicon oxide material with polymer microsphere emulsion and spray drying and heating carbonization, a coated silicon oxide composite material is formed, which solves the structural damage caused by the change in the volume of silicon-based materials in lithium-ion batteries. and resource waste issues have improved the battery's high-temperature cycle performance and resource utilization rate.

CN115911295BActive Publication Date: 2024-11-19ZHEJIANG LICHEN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211181292.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-11-19
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

The volume expansion and contraction of silicon-based materials in existing lithium-ion batteries leads to structural damage during lithium embedding and deliquification, affecting battery life, and the accumulation of fine powder of silicon oxide material leads to waste of resources and affecting battery performance.

Method used

The fine powder of silicon oxide material is blended with polymer microsphere emulsion, and the coated silicon oxide composite material is formed by spray drying and heating and carbonization, which improves its high-temperature cycling performance and resource utilization in lithium-ion batteries.

Benefits of technology

It has achieved the improvement of high-temperature cycling performance of lithium-ion batteries and the effective utilization of resources, extended battery life, and improved the first-time Coulomb efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115911295B_ABST
    Figure CN115911295B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a silicon oxide composite material, which uses silicon oxide material fine powder with a median particle size of 0.1 to 2.0 μm as a raw material, firstly forms a granulation slurry by compounding it with a polymer microsphere emulsion of a special composition, and then spray-drying it. During the treatment process, secondary granulation of the silicon oxide material fine powder and polymer coating of the silicon oxide material after the secondary granulation are simultaneously achieved, and finally heating and carbonization are performed. The preparation method of the invention effectively solves the problem of serious waste of resources caused by large-scale accumulation of silicon oxide material fine powder; the prepared silicon oxide composite material has a suitable median particle size and specific surface area, and the carbon layer coated on the surface is also extremely uniform. The lithium ion battery assembled with it as the negative electrode material has excellent high-temperature cycle performance, and has both high capacity and high first coulomb efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a silicon oxide composite material, a product thereof and an application of the same in lithium ion batteries. Background Art

[0002] Lithium-ion batteries are widely used in various portable electronic devices and electric vehicles due to their advantages such as high specific energy, high operating voltage, long cycle life and low self-discharge rate, which has changed the modern way of life and production of human beings. At present, the negative electrode materials of commercial lithium-ion batteries are mainly graphite, including natural graphite and artificial graphite, in addition to soft carbon and hard carbon, etc. However, because the theoretical capacity of graphite is only 372mAh / g, it can no longer meet the demand for high energy density power sources in the application field of lithium-ion batteries. Therefore, there is an urgent need to develop a new type of high specific capacity lithium-ion battery negative electrode material.

[0003] Silicon-based materials have always attracted much attention as negative electrode materials for lithium-ion batteries. Silicon-based materials use an alloying reaction process to store energy. When used as negative electrode materials, they have an ultra-high theoretical specific capacity of 4200mAh / g, which is more than 10 times the capacity of commercialized graphite negative electrodes. In addition, they have the advantages of low lithium insertion potential, low price and environmental friendliness. Therefore, silicon-based materials are a strong candidate for the new generation of high-capacity negative electrode materials. However, since the volume of silicon-based materials will expand and contract rapidly during the process of lithium ion insertion and extraction, with an expansion rate of 100-300%, the continuous expansion and contraction will cause the structure of silicon-based materials to be destroyed and pulverized, and it is difficult to form a stable SEI film. After multiple cycles, the capacity decays severely, resulting in a significant decrease in the overall performance of the battery, seriously affecting the battery life and limiting its commercial application.

[0004] Among silicon-based materials, silicon oxide material is a negative electrode material with a higher specific capacity. At the same time, compared with silicon alone, its volume change during the charge and discharge process is smaller. This is because during the first lithium insertion process, silicon oxide material is lithiated to generate active silicon, lithium oxide and lithium silicate. The active silicon generated in situ is dispersed in the lithium oxide-lithium silicate amorphous matrix. Such a structure can buffer the volume change caused by the active silicon deintercalation process. In addition, silicon oxide material also has the advantages of low operating voltage, good safety and wide source of raw materials. Therefore, silicon oxide material has become a hot topic for researchers in recent years.

[0005] During the preparation of silicon oxide materials, silicon oxide material fine powder (median particle size D50 is about 0.1-2.0μm) will be produced. Compared with silicon oxide materials of normal particle size (median particle size D50 is about 6-8μm), silicon oxide material fine powder has a larger specific surface area. When used as a negative electrode material for lithium-ion batteries to insert lithium, the area of ​​the formed SEI film will increase, and a large amount of electrolyte will be consumed, which will lead to a decrease in the high-temperature cycle performance of the battery. At the same time, in the process of making electrode sheets, silicon oxide material fine powder is easy to agglomerate uncontrollably, resulting in poor processing performance of the electrode sheets. If it is not utilized, a large amount of accumulation will occur after continuous accumulation, resulting in a serious waste of resources. Therefore, a technology is urgently needed to solve this problem. Summary of the invention

[0006] In view of the above problems existing in the prior art, the present invention discloses a method for preparing a silicon oxide composite material. The silicon oxide material fine powder is directly used as a raw material. The lithium-ion battery assembled with the prepared silicon oxide composite material has excellent high-temperature cycle performance, and has both high capacity and high first coulombic efficiency; and effectively solves the problem of serious waste of resources caused by large-scale accumulation of silicon oxide material fine powder.

[0007] The specific technical solutions are as follows:

[0008] A method for preparing a silicon oxide composite material comprises the following steps:

[0009] (1) dispersing silicon dioxide material fine powder in deionized water to obtain a suspension;

[0010] The median particle size of the silicon oxide material fine powder is 0.1 to 2.0 μm;

[0011] (2) blending the suspension with the polymer microsphere emulsion to obtain a uniformly mixed slurry for granulation;

[0012] The polymer microsphere emulsion is prepared by polymerization of monomer A, monomer B and amino-containing monomer C as raw monomers initiated by an initiator;

[0013] The A monomer is selected from styrene monomers;

[0014] The B monomer is selected from one or more of acrylate monomers, methacrylate monomers, acrylonitrile, and methacrylonitrile;

[0015] The amino-containing C monomer is selected from one or more of acrylamine, acrylamide, methacrylamide, and ethyleneimine;

[0016] (3) spray drying the granulation slurry to obtain a coated silicon oxide material precursor;

[0017] (4) The coated silicon iodine oxide material precursor is subjected to a heating and carbonization treatment to obtain the silicon iodine oxide composite material.

[0018] The preparation method disclosed in the present invention directly uses silicon oxide material powder with a median particle size of 0.1 to 2.0 μm as raw material, firstly forms a granulation slurry by compounding it with a polymer microsphere emulsion of a special composition, and then spray-drying it. During the treatment process, secondary granulation of the silicon oxide material powder and polymer coating of the silicon oxide material after the secondary granulation are simultaneously achieved, and finally the silicon oxide composite material is obtained by heating and carbonization.

[0019] The experiment found that the composition of the polymer microsphere emulsion in the preparation method is particularly critical. The raw material composition includes three monomers, namely, A monomer selected from styrene monomers, B monomer selected from one or more of acrylate monomers, methacrylate monomers, acrylonitrile, and methacrylonitrile, and C monomer containing an amino group. A monomer can improve the bonding force with the fine powder of silicon dioxide material, help to form a coating layer, and after high-temperature treatment, it is more conducive to forming a carbon layer structure in the form of a single-layer particle, uniformly coating the surface of the silicon dioxide material, and improving the charge and discharge cycle performance; B monomer can give the polymer microspheres good lithium ion conductivity, and at the same time can enhance the bonding force between the negative electrode active particles and the current collector; and the introduction of C monomer containing an amino group can further regulate the glass transition temperature (T g ), so as to match the process conditions of spray drying. During spray drying, the fine powder of silicon oxide material can be secondary granulated, and the secondary particles of silicon oxide material with suitable particle size can be obtained. All three are indispensable, otherwise the median particle size of the prepared silicon oxide composite material will be too large or too small, thereby affecting the electrochemical performance of the lithium ion battery assembled therefrom.

[0020] In step (1):

[0021] The median particle size of the silicon nitride material powder is 0.5 to 2.0 μm; preferably, the median particle size of the silicon nitride material powder is 0.5 to 1.5 μm; more preferably, the median particle size is 1.5 μm.

[0022] Silicon oxide material, its structural formula is SiO x , x is selected from 0.8 to 1.5, preferably, x is selected from 1.0.

[0023] The solid content of the suspension is 1 to 30 wt %, preferably 5 to 15 wt %, and more preferably 8 to 10 wt %.

[0024] In step (2):

[0025] The styrene monomer is selected from one or more of styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2-fluorostyrene, 3-fluorostyrene, and 4-fluorostyrene; preferably, the A monomer is selected from styrene.

[0026] The acrylic acid ester monomer is selected from one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, nonyl acrylate, and decyl acrylate;

[0027] The methacrylate monomer is selected from one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, nonyl methacrylate, and decyl methacrylate;

[0028] Preferably, the B monomer is selected from acrylate monomers and / or methacrylate monomers.

[0029] The initiator is selected from the common initiator types in the art, such as azo initiators and peroxide initiators.

[0030] The azo initiator is selected from azobisisobutyronitrile, azobisisoheptanenitrile, etc.;

[0031] The peroxide initiator is selected from hydroperoxides, acyl peroxides, dialkyl peroxides, ester peroxides, ketone peroxides, dicarbonate peroxides, etc., specifically tert-butyl hydroperoxide, isopropylbenzene hydroperoxide, benzoyl peroxide BPO, dodecyl peroxide LPO, lauroyl peroxide, diisopropyl peroxide, tert-butyl perbenzoate, tert-butyl pervalerate, methyl ethyl ketone peroxide, cyclohexanone peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, etc.

[0032] The polymerization may be any one of solution polymerization, emulsion polymerization, precipitation polymerization and suspension polymerization, and the specific polymerization process adopts conventional technical means in the art.

[0033] The solid content of the polymer microsphere emulsion is 20-60 wt %, and the solid content of the polymer microsphere emulsion is adjusted by adding water.

[0034] Based on the total dry weight of the polymer microsphere emulsion as 100 parts, the raw material composition includes:

[0035]

[0036] Preferably, the raw material composition includes:

[0037]

[0038] Further preferably, the raw material composition comprises:

[0039]

[0040] Still more preferably, based on the total dry weight of the polymer microsphere emulsion as 100%, the raw material composition includes:

[0041]

[0042] More preferably, the raw material composition includes 5% of C monomer containing amino group.

[0043] Experiments have shown that with the continuous optimization of the raw material composition in the polymer microsphere emulsion, the glass transition temperature of the prepared polymer microspheres is better matched with the process parameters of spray drying. The D50 of the finally prepared silicon dioxide composite material is about 6 to 12 μm, and it has better electrochemical properties when used as a negative electrode material.

[0044] Preferably, the mass ratio of the silicon oxide material powder added in step (1) to the dry weight of the polymer microsphere emulsion added in step (2) is 1:0.1-0.3. It has been found through experiments that the use of this ratio can ensure that the polymer microspheres are coated in the form of a single layer on the surface of the prepared silicon oxide material secondary particles, and after heating and carbonization treatment, the carbon layer can be evenly coated on the surface of the secondary particles; by adjusting this ratio, the thickness of the carbon layer coated in the finally prepared silicon oxide composite material can also be adjusted. When the ratio of the two is too low, that is, the dry weight of the added polymer microsphere emulsion is too much, it may cause the polymer microspheres to agglomerate and fail to be coated in the form of a single layer, which in turn causes the thickness of the coated carbon layer to be uneven.

[0045] More preferably, the dry weight ratio of the silicon dioxide material fine powder added in step (1) to the polymer microsphere emulsion added in step (2) is 1:0.2.

[0046] In the present invention, the dry weight in the polymer microsphere emulsion is the product of the total mass of the polymer microsphere emulsion and the solid content.

[0047] In step (3):

[0048] When spray drying silicon dioxide materials, it is necessary to consider the problem that the spray drying temperature is too low, resulting in the inability to completely dry the material, and the problem that the spray drying temperature is too high may change the properties of the material itself, such as oxidation, and the energy consumption is too high. Therefore, after comprehensive consideration, the spray drying is controlled, and the air inlet temperature is 160-220°C, and more preferably 180-200°C. It is found through experiments that the polymer microsphere emulsion composed of the above special raw materials can improve the T of the polymer microspheres coated on the surface of the silicon dioxide material fine powder. g When the process parameters are adjusted to match the spray drying process parameters, the D50 of the silicon dioxide composite material finally prepared can be further affected, and the D50 can be controlled within the range of 4.5 to 13.5 μm.

[0049] Preferably, during the spray drying process, the feed rate is 0.01 to 2.5 kg / min and the air pressure is 0.1 to 1.0 MPa.

[0050] In step (4):

[0051] The heating carbonization treatment is carried out under an inert atmosphere, firstly heating to 250-400° C., keeping the temperature for 0.5-4.0 hours, then heating to 750-1100° C., keeping the temperature for 2-20 hours.

[0052] The experiment found that compared with the single heating, the secondary heating can reduce the specific surface area of ​​the prepared silicon dioxide composite material, and the assembled lithium-ion battery has a higher high-temperature cycle capacity retention rate and a higher specific capacity.

[0053] The inert atmosphere is selected from one or more of nitrogen, helium, neon and argon.

[0054] Preferably, the heating rate is selected from 3 to 10° C. / min.

[0055] The present invention also discloses a silicon oxide composite material prepared according to the above method, comprising secondary particles of silicon oxide material and a pyrolytic carbon layer covering the secondary particles of silicon oxide material.

[0056] Preferably, the median particle size of the silicon oxide composite material is 4.5 to 15 μm, more preferably 4.5 to 13.5 μm, and even more preferably 6 to 12 μm.

[0057] Preferably, the thickness of the pyrolytic carbon layer is 5 to 10 nm.

[0058] Preferably, the specific surface area of ​​the silicon oxide composite material is 1 to 4 m 2 / g, more preferably 2 to 3 m 2 / g.

[0059] The present invention also discloses the use of the silicon dioxide composite material in the preparation of lithium-ion batteries. The assembled lithium-ion batteries have excellent high-temperature (60° C.) cycle performance and have both high capacity and high first coulombic efficiency.

[0060] Compared with the prior art, the present invention has the following beneficial effects:

[0061] The invention discloses a method for preparing a silicon oxide composite material, which directly uses silicon oxide material fine powder as raw material, effectively solving the problem of serious waste of resources caused by large-scale accumulation of silicon oxide material fine powder; the prepared silicon oxide composite material has a suitable median particle size and specific surface area, and the carbon layer coated on the surface is also extremely uniform. The lithium ion battery assembled with the silicon oxide composite material as the negative electrode material has excellent high-temperature cycle performance, and has both high capacity and high first coulombic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is a SEM image of the coated silicon dioxide material precursor prepared in step (4) of Example 1;

[0063] Figure 2 TEM image of the silicon dioxide composite material prepared in Example 1;

[0064] Figure 3 is the DSC curve of the polymer microspheres in the polymer microsphere emulsion prepared in step (2) in Example 1;

[0065] Figure 4 The DSC curve of the polymer microspheres in the polymer microsphere emulsion prepared in step (2) of Comparative Example 4;

[0066] Figure 5 TEM image of the silicon dioxide composite material prepared in Comparative Example 5;

[0067] Figure 6 This is the first charge and discharge curve of a button battery assembled using the silicon dioxide composite material prepared in Example 1 as the negative electrode material;

[0068] Figure 7 This is the cycle curve of a small soft-pack battery assembled with the silicon dioxide composite material prepared in Example 1 as the negative electrode material. DETAILED DESCRIPTION

[0069] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below in conjunction with the embodiments and drawings. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0070] The performance parameters of the intermediate products and final products in the following examples and comparative examples are measured according to the following methods.

[0071] 1. Median particle size D50: measured using a laser particle size analyzer (Malvern Mastersizer 2000).

[0072] 2. Glass transition temperature T g : The polymer microsphere emulsion was first dried in a vacuum drying oven at 100°C to obtain a solid substance, and then tested using a differential scanning calorimeter (DSC).

[0073] 3. Specific surface area BET: measured using a BET specific surface area tester (TriStar II 3020).

[0074] Example 1

[0075] (1) Preparation of silicon oxide fine powder suspension

[0076] 100 g of silicon dioxide material powder SiO (D50 is 1.5 μm, purchased from Yunnan Lichen New Material Technology Co., Ltd.) was added to 1.0 kg of deionized water, and the mixture was fully stirred and dispersed for 2 h to obtain a suspension of silicon dioxide material powder, wherein the solid content of the suspension was 9.09%.

[0077] (2) Preparation of polymer microsphere emulsion

[0078] Based on 100 parts of total dry weight, 100 parts of deionized water were added to the emulsion reactor, the temperature was raised to 75°C, 0.5 parts of a 20% deionized ammonium persulfate solution by mass (equivalent to 0.1 parts of ammonium persulfate by dry weight) was added, and then 40.0 parts of styrene, 54.90 parts of ethyl acrylate, and 5.0 parts of acrylamide were added to the reactor, stirred and blended at 600 rpm, and added at a uniform speed for 3 hours. After the addition, the reaction was continued for 2 hours, and then vacuumed to -75 kPa. The reaction was carried out under this condition for 1.5 hours, and finally cooled to below 45°C to stop the reaction, and passed through a 100-mesh sieve to obtain a polymer microsphere emulsion, and 50 parts of deionized water were added to adjust the solid content of the finally prepared polymer microsphere emulsion to 40%.

[0079] The median particle size D50 of the polymer microspheres in the prepared polymer microsphere emulsion was measured by a laser particle size analyzer to be 0.35 μm. The prepared polymer microsphere emulsion was dried at 100° C. in a vacuum drying oven to a solid substance, and then sintered at 1200° C. in a nitrogen atmosphere for 2 hours. After testing, the residual carbon content was 32.6%.

[0080] The glass transition temperature T of the polymer microspheres in the prepared polymer microsphere emulsion was determined by DSC. gis 214℃, DSC graph is as follows Figure 3 shown.

[0081] (3) Preparation of slurry for granulation

[0082] 50 g of the polymer microsphere emulsion prepared in step (2) (equivalent to 20 g of dry weight) was added to the suspension prepared in step (1), and stirred at 75° C. and 600 rpm for 0.5 hour to prepare a granulation slurry having a solid content of 10.4%.

[0083] (4) Preparation of coated silicon oxide material precursor

[0084] Using a spray dryer, setting the inlet air temperature to 200° C., the exhaust air temperature to 70° C., the feed rate to 0.1 kg / min, the gas pressure to 0.2 MPa, and the rotation frequency to 40 Hz, the granulation slurry prepared in step (3) is spray-dried to obtain a granulated and coated powder material, i.e., a coated silicon dioxide material precursor;

[0085] (5) Preparation of silicon dioxide composite materials

[0086] The precursor prepared in step (4) is loaded into a crucible with a filling amount of 50wt%. Under the protection of a nitrogen atmosphere, the temperature is increased to 320°C at a heating rate of 8°C / min, and the temperature is kept for 2h. Then, the temperature is increased to 900°C at a heating rate of 8°C / min, and the temperature is kept for 5h. The crucible is naturally cooled and the silicon dioxide composite material is collected.

[0087] Figure 1 This is the SEM image of the coated silicon dioxide material precursor prepared in step (4) of this embodiment. By observing the image, it can be found that the polymer microspheres are coated on the surface of the prepared silicon dioxide material secondary particles in the form of a single layer, and after heating and carbonization treatment, the carbon layer can be evenly coated on the surface of the secondary particles.

[0088] Figure 2 This is a TEM image of the silicon oxide composite material prepared in this example at a high magnification. From the image, it can be observed that the carbon layer is very evenly coated on the surface of the secondary particles of the silicon oxide material, and it can be found that the thickness of the carbon coating layer is 5.5 nm.

[0089] After testing, the D50 of the silicon dioxide composite material finally prepared in this embodiment is 6.52 μm; the specific surface area is 2.54 m 2 / g.

[0090] Example 2

[0091] The preparation process is basically the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 42.5 parts of styrene, 56.9 parts of ethyl acrylate and 0.5 parts of acrylamide.

[0092] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0093] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0094] Example 3

[0095] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 35.0 parts of styrene, 49.9 parts of ethyl acrylate and 15.0 parts of acrylamide.

[0096] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0097] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0098] Example 4

[0099] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 42.0 parts of styrene, 55.9 parts of ethyl acrylate and 2 parts of acrylamide.

[0100] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0101] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0102] Example 5

[0103] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 38.0 parts of styrene, 53.9 parts of ethyl acrylate and 8.0 parts of acrylamide.

[0104] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0105] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0106] Example 6

[0107] The preparation process is substantially the same as that of Example 1, except that in step (2), the added styrene is replaced by an equal weight portion of 2-methylstyrene.

[0108] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0109] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0110] Example 7

[0111] The preparation process is basically the same as that of Example 1, except that in step (2), the added styrene is replaced by an equal weight portion of 3-chloro-styrene.

[0112] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0113] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0114] Example 8

[0115] The preparation process is basically the same as that of Example 1, except that in step (2), the added ethyl acrylate is replaced by an equal weight portion of decyl methacrylate.

[0116] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0117] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0118] Example 9

[0119] The preparation process is basically the same as that of Example 1, except that in step (2), the added ethyl acrylate is replaced by an equal weight portion of acrylonitrile.

[0120] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0121] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0122] Example 10

[0123] The preparation process is substantially the same as that of Example 1, except that in step (2), the added acrylamide is replaced by an equal weight portion of ethyleneimine.

[0124] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0125] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0126] Embodiment 11

[0127] The preparation process is basically the same as that of Example 1, except that in step (3), 75 g of the polymer microsphere emulsion prepared in step (2) (equivalent to 30 g in dry weight) is added.

[0128] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0129] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0130] The coated silicon monoxide material precursor prepared in step (4) was characterized by SEM, and it can be observed that the polymer microspheres are still uniformly coated on the surface of the prepared silicon monoxide material secondary particles in the form of a single layer.

[0131] TEM characterization shows that the carbon layer coated on the surface of the silicon oxide composite material prepared in this example is very uniform, and the thickness of the carbon layer is about 10 nm.

[0132] Example 12

[0133] The preparation process is basically the same as that of Example 1, except that in step (1), the silicon monoxide material powder with a D50 of 1.5 μm is replaced with silicon monoxide material powder with an equal mass and a D50 of 0.5 μm.

[0134] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0135] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0136] Example 13

[0137] The preparation process is basically the same as that of Example 1, except that in step (1), the silicon monoxide material powder with a D50 of 1.5 μm is replaced with silicon monoxide material powder with an equal mass and a D50 of 2.0 μm.

[0138] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0139] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0140] Embodiment 14

[0141] The preparation process is basically the same as that of Example 1, except that in step (4), the inlet air temperature is replaced with 184°C.

[0142] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0143] Embodiment 15

[0144] The preparation process is basically the same as that of Example 1, except that in step (4), the inlet air temperature is replaced with 164°C.

[0145] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0146] Example 16

[0147] The preparation process is basically the same as that of Example 1, except that in step (1), 100 g of silicon dioxide powder is replaced with an equal mass of SiO 0.8 (D50 is 1.5 μm, purchased from Yunnan Lichen New Materials Technology Co., Ltd.).

[0148] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0149] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0150] Embodiment 17

[0151] The preparation process is basically the same as that of Example 1, except that in step (1), 100 g of silicon dioxide powder is replaced with an equal mass of SiO 1.5 (D50 is 1.5 μm, purchased from Yunnan Lichen New Materials Technology Co., Ltd.).

[0152] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this example is g The data are listed in Table 1 below.

[0153] The D50 and specific surface area of ​​the silicon dioxide composite material prepared in this example are also listed in Table 1 below.

[0154] Comparative Example 1

[0155] Take 1.0 kg of fine powder of silicon dioxide material (D50 is 1.5 μm) and place it in a chemical vapor deposition furnace. First, introduce nitrogen to maintain an inert atmosphere in the furnace. Set the temperature to 600°C at a rate of 5°C / min, then introduce acetylene gas. The flow rate ratio of acetylene gas to nitrogen is 1:3. Continue to heat to 900°C and keep it at this temperature for 3 hours for vapor deposition to obtain gas-phase carbon-coated silicon dioxide material.

[0156] The D50 and specific surface area of ​​the silicon-based composite material prepared in this comparative example are listed in the following Table 1.

[0157] Comparative Example 2

[0158] The preparation process is substantially the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 94.9 parts of styrene and 5 parts of acrylamide.

[0159] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this comparative example is g The data are listed in Table 1 below.

[0160] The D50 and specific surface area of ​​the silicon-based composite material prepared in this comparative example are also listed in the following Table 1.

[0161] Comparative Example 3

[0162] The preparation process is basically the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 94.9 parts of ethyl acrylate and 5 parts of acrylamide.

[0163] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this comparative example is g The data are listed in Table 1 below.

[0164] The D50 and specific surface area of ​​the silicon-based composite material prepared in this comparative example are also listed in the following Table 1.

[0165] Comparative Example 4

[0166] The preparation process is basically the same as that of Example 1, except that in step (2), the monomer raw materials added to the reactor are 40 parts of styrene and 59.90 parts of ethyl acrylate.

[0167] Figure 4 This is the DSC curve of the polymer microspheres prepared in this comparative example. From the figure, it can be found that the glass transition temperature of the polymer microspheres is 118°C.

[0168] The D50 and specific surface area of ​​the silicon-based composite material prepared in this comparative example are listed in the following Table 1.

[0169] Comparative Example 5

[0170] The preparation process is basically the same as that of Example 1, except that in step (3), 100 g of the polymer microsphere emulsion prepared in step (2) (equivalent to 40 g in dry weight) is added.

[0171] Figure 5 This is a TEM image of the silicon oxide composite material prepared in this comparative example at a high magnification. From the image, it can be observed that the carbon layer is unevenly coated on the surface of the secondary particles of the silicon oxide material.

[0172] The D50 and specific surface area of ​​the silicon-based composite material prepared in this comparative example are listed in the following Table 1.

[0173] Comparative Example 6

[0174] The preparation process is basically the same as that of Example 1, with the only difference being that in step (5), the secondary heating is replaced by a single heating, specifically, the temperature is directly increased to 900° C. at a heating rate of 8° C. / min and kept at this temperature for 5 h.

[0175] The glass transition temperature T of the polymer microspheres in the polymer microsphere emulsion prepared in this comparative example is g The data are listed in Table 1 below.

[0176] The D50 and specific surface area of ​​the silicon-based composite material prepared in this comparative example are also listed in the following Table 1.

[0177] Table 1

[0178]

[0179] Performance Test:

[0180] 1. The silicon-based composite materials prepared in Examples 1 to 17 and Comparative Examples 1 to 6 were used as negative electrode materials to prepare model 2032 button batteries. The specific steps are as follows: the silicon-based composite material, the conductive agent SP, the dispersant CMC, and the binder AONE were mixed in a mass ratio of 70:15:5:10, and water was used as a solvent to prepare a negative electrode slurry; the negative electrode slurry was coated on a copper foil, and a lithium sheet was used as a counter electrode and a Celgard 2400 microporous polypropylene film was used as a separator to prepare a button battery.

[0181] The prepared button battery was subjected to charge and discharge cycles, and the charge and discharge conditions were as follows:

[0182] The charge and discharge cut-off voltage is 0.005-1.5V. The discharge rate is 0.1C to 0.005V, and then 0.02C to 0.005V to fully discharge it. The charge rate is 0.1C to 1.5V. The reversible capacity and first coulomb efficiency of the button battery are tested. The results are shown in Table 2 below.

[0183] The first charge and discharge curve of the button battery assembled in Example 1 is shown in Figure 6 .

[0184] 2. The silicon-based composite materials prepared in Examples 1 to 17 and Comparative Examples 1 to 6 were used as negative electrode materials to prepare small soft-pack batteries, and the specific steps were as follows:

[0185] The silicon oxide composite negative electrode material and commercial artificial graphite (Yunnan Zhongsheng) were mixed in a mass ratio of 8.1:91.9 to form an active material with a capacity of 450mAh / g. The active material, binder lithium polyacrylate and conductive agent Super P were dispersed and slurried in a mass ratio of 95.5:4:0.5. After coating, rolling, slitting and other battery preparation processes, and matched with NCM811 positive electrode, a small soft-pack battery was made.

[0186] High temperature cycle performance test: At 60°C, charge the battery to 4.2V at 0.5C constant current and constant voltage, cut off current 0.02C, leave for 5 minutes, then discharge to 2.5V at 1C constant current, leave for 5 minutes. After 300 cycles of charge / discharge, calculate the 300th cycle capacity retention rate. The calculation formula is as follows:

[0187] The 300th cycle capacity retention rate at high temperature (%) = (300th cycle reversible capacity / 1st cycle reversible capacity) × 100%.

[0188] Figure 7 This is the cycle stability curve of the small soft-pack battery assembled in Example 1. The capacity retention rate data of the small soft-pack batteries assembled in each example and each comparative example at the 300th cycle at high temperature are listed in the following Table 2.

[0189] Table 2

[0190]

[0191]

Claims

1. A method for preparing a silicon oxide composite material, characterized in that: The steps include: (1) dispersing silicon dioxide material fine powder in deionized water to obtain a suspension; The median particle size of the silicon oxide material fine powder is 0.1-2.0 μm; (2) blending the suspension with the polymer microsphere emulsion to obtain a uniformly mixed slurry for granulation; The polymer microsphere emulsion is prepared by polymerization of monomer A, monomer B and amino-containing monomer C as raw monomers initiated by an initiator; The A monomer is selected from styrene monomers; The B monomer is selected from one or more of acrylate monomers, methacrylate monomers, acrylonitrile, and methacrylonitrile; The amino-containing C monomer is selected from one or more of acrylamine, acrylamide, methacrylamide, and ethyleneimine; The solid content of the polymer microsphere emulsion is 20-60wt%. Based on 100 parts of the total dry weight of the polymer microsphere emulsion, the raw material composition includes: 10-50 parts of A monomer; 24 to 89 parts of B monomer; 0.5-25.0 parts of amino-containing C monomer; Initiator 0.001~2.0 parts; The dry weight ratio of the silicon dioxide material fine powder added in step (1) to the polymer microsphere emulsion added in step (2) is 1:0.1-0.3; (3) spray drying the granulation slurry to obtain a coated silicon oxide material precursor; (4) The coated silicon oxide material precursor is subjected to a heating and carbonization treatment to obtain the silicon oxide composite material.

2. The method for preparing the silicon dioxide composite material according to claim 1, characterized in that: In step (1): The median particle size of the silicon oxide material fine powder is 0.5-2.0 μm; The solid content of the suspension is 1-30 wt %.

3. The method for preparing the silicon dioxide composite material according to claim 1, characterized in that: In step (2): The styrene monomer is selected from one or more of styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2-fluorostyrene, 3-fluorostyrene, and 4-fluorostyrene; The acrylic acid ester monomer is selected from one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, nonyl acrylate, and decyl acrylate; The methacrylate monomer is selected from one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, nonyl methacrylate and decyl methacrylate.

4. The method for preparing the silicon dioxide composite material according to claim 3, characterized in that: Based on the total dry weight of the polymer microsphere emulsion as 100 parts, the raw material composition includes: 35-45 parts of A monomer; 45-60 parts of B monomer; 0.5-15.0 parts of amino-containing C monomer; Initiator 0.01~2.0 parts.

5. The method for preparing the silicon dioxide composite material according to claim 4, characterized in that: Based on the total dry weight of the polymer microsphere emulsion as 100 parts, the raw material composition includes: 35-45 parts of A monomer; 45-60 parts of B monomer; 2-8 parts of amino-containing C monomer; Initiator 0.01~2.0 parts.

6. The method for preparing the silicon dioxide composite material according to claim 1, characterized in that: In step (2): The A monomer is selected from styrene; The B monomer is selected from acrylate monomers and / or methacrylate monomers; The amino-containing C monomer is selected from acrylamide.

7. The method for preparing the silicon dioxide composite material according to claim 1, characterized in that: In step (3): The spray drying has an air inlet temperature of 160-220°C and an air pressure of 0.1-1.0 MPa; In step (4): The heating carbonization treatment is carried out under an inert atmosphere, firstly heating to 250-400° C., keeping the temperature for 0.5-4.0 hours, then heating to 750-1100° C., keeping the temperature for 2-20 hours.

8. A silicon oxide composite material prepared according to the method according to any one of claims 1 to 7, characterized in that: The invention relates to secondary particles comprising silicon oxidized material and a pyrolytic carbon layer covering the secondary particles of silicon oxidized material.

9. The silicon dioxide composite material according to claim 8, characterized in that: The median particle size of the silicon oxide composite material is 4.5-15 μm; The thickness of the pyrolytic carbon layer is 5-10 nm; The specific surface area of ​​the silicon oxide composite material is 1 to 4 m 2 / g.

10. Use of the silicon dioxide composite material according to claim 8 or 9 in preparing a lithium ion battery.