A method for preparing tetrahedral mesoporous CuPd catalyst
By preparing tetrahedral mesoporous CuPd catalyst in direct ethylene glycol fuel cell, the problems of weak catalytic activity, low selectivity and poor stability in ethylene glycol oxidation reaction are solved by using bromide ion induction and intrinsic activity of bimetallic alloys. , achieving efficient electrocatalytic effect.
Patent Information
- Application Number
- CN202211664511.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-23
AI Technical Summary
In the anode semi-reaction of direct ethylene glycol fuel cell, the catalytic activity, low selectivity and poor stability during the ethylene glycol oxidation reaction, and existing catalysts are difficult to effectively promote the reaction.
The tetrahedral mesoporous CuPd catalyst was prepared by a simple liquid phase method, and the co-assembly and co-reduction of asymmetric morphology was achieved by bromide ion induction, combining the intrinsic activity of copper and palladium two-component alloys to optimize the structure and components of the catalyst. Improve catalytic activity and selectivity.
It has achieved a significant improvement in catalytic activity, selectivity and stability in the electrocatalytic oxidation reaction of glycol, reduced the cost of catalyst preparation, and is suitable for large-scale industrial production.
Smart Images

Figure CN115911417B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and in particular relates to a method for preparing a tetrahedral mesoporous metal catalyst for ethylene glycol electrocatalytic oxidation reaction. Background Art
[0002] Alkaline direct fuel cells are considered to be a very promising energy device that can convert chemical energy into electrical energy. For example, hydrogen and alcohol are commonly used as fuels for fuel cells. Compared with hydrogen, methanol, and ethanol, ethylene glycol has higher theoretical energy density and advantages such as low toxicity, high boiling point, and safe storage. However, due to the lack of suitable and efficient electrocatalysts, the ethylene glycol oxidation reaction process in the anode half reaction of direct ethylene glycol fuel cells (i.e., ethylene glycol oxidation reaction (EGOR)) is still limited by electrocatalytic reaction kinetics and severe intermediate poisoning. In this regard, many researchers have made efforts to overcome this by precisely manipulating the morphology / structure and crystallinity of metal nanocatalysts, which kinetically promote the removal of toxic intermediates and promote CC bond cleavage during the EGOR electrocatalytic process, but the performance gain is still unsatisfactory.
[0003] Since the first discovery of MCM-41 in 1992, ordered mesoporous materials have received increasing attention in various applications. As second-generation mesoporous materials, mesoporous metals with a continuous crystalline framework have special application value in catalysis and electrocatalysis. In general, mesoporous metals have multiple advantages of "large nanoparticles" with fast electron transfer and high stability and "small nanoparticles" with large surface area and many catalytic active sites, which significantly improve their (electro)catalytic performance. More interestingly, the crystalline mesoporosity of mesoporous metals can optimize their electronic and spatial structures and provide a nanoscale confined environment, which has the potential to adjust their (electro)catalytic selectivity for certain specific products.
[0004] Controlling the shape of nanocrystals is a simple and effective means to tailor their properties and optimize their performance in various applications. To this end, many studies have reported the preparation of noble metal nanocrystals with a variety of different shapes (e.g., spheres, cubes, octahedra, and plates). However, due to the inherent face-centered cubic (fcc) lattice of noble metals, basically all of these shapes are highly symmetrical spatial arrangements of atoms. If the symmetry can be broken in a controlled way, it is possible to obtain nanocrystals with certain shapes, and even further predict properties that have never been explored before. However, most of the current mechanisms for the design and synthesis of asymmetric metal crystals need to be improved, not to mention the very limited number of asymmetric shapes. Breaking the asymmetry based on the metal particle scale is already very challenging, not to mention metal crystals with mesoporous channels. The synthesis of asymmetric mesoporous metals with broken metal symmetry and specific morphologies is expected, because asymmetric mesoporous crystals are expected to exhibit unique physicochemical properties that are different from symmetric mesoporous metal crystals, especially based on the unique structural advantages of asymmetric mesoporous crystals in (electro)catalytic reactions. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of weak catalytic activity, low selectivity and poor stability in the electrocatalytic oxidation reaction of ethylene glycol, and to provide a method for preparing a tetrahedral mesoporous metal catalyst for efficient electrocatalytic oxidation of ethylene glycol. The present invention realizes the preparation of mesoporous metal nanoparticles with tetrahedral morphology through a simple liquid phase method, and combines the synergistic kinetic diffusion advantages of tetrahedral structure and mesoporous structure, as well as the intrinsic activity of copper and palladium two-component alloy, so that it exhibits excellent catalytic activity, selectivity and stability in the electrocatalytic oxidation reaction of ethylene glycol.
[0006] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: a cationic surfactant is dissolved in deionized water, and the pH is adjusted to 10 to 12, then a structure inducer, chloropalladic acid and copper nitrate are added, the obtained reaction solution is allowed to stand for reaction at 40 to 60° C. for 30 to 60 minutes, L-ascorbic acid is added, and the reaction is allowed to stand for reaction at 40 to 60° C. for 2 to 3 hours, centrifuged and washed, and vacuum dried to obtain a tetrahedral mesoporous CuPd catalyst; wherein the cationic surfactant is any one or two of hexadecyltrimethylammonium chloride (CTAC) and hexadecyltrimethylammonium bromide (CTAB); and the structure inducer is any one or more of potassium bromide, sodium bromide and ammonium bromide.
[0007] In the above preparation method, the amount of the cationic surfactant added to the deionized water is preferably 1.5 to 3 mg / mL.
[0008] In the above preparation method, it is preferred to adjust the pH to 10-12 using 0.1 mol / L sodium hydroxide or potassium hydroxide aqueous solution.
[0009] In the above preparation method, preferably, the concentration of the structure inducing agent in the reaction solution is 0.005-0.01 mol / L, the concentration of chloropalladic acid is 0.5-1.5 mmol / L, and the concentration of copper nitrate is 0.5-1.5 mmol / L.
[0010] In the above preparation method, the added amount of the L-ascorbic acid is preferably 15 to 30 times the total molar amount of chloropalladic acid and copper nitrate.
[0011] In the above preparation method, preferably, the molar ratio of Pd to Cu in the tetrahedral mesoporous CuPd catalyst is 90:10 to 50:50.
[0012] In the above preparation method, it is preferred to perform centrifugal washing with ethanol and dry in a vacuum oven at 40-60° C. to remove the cationic surfactant.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] 1. The present invention uses bromide ions to modify cationic surfactants and then adds metal precursors chloropalladic acid and copper nitrate, and uses electrostatic interaction and bromide ion induction to achieve co-assembly of surfactant-metal precursors; then adds co-reducing agent L-ascorbic acid to achieve co-reduction along the assembled surfactant-metal precursor to obtain a tetrahedral mesoporous CuPd catalyst. The preparation of the tetrahedral mesoporous CuPd catalyst of the present invention has three unique advantages: (i) bromide ions are used as inducers to achieve the successful preparation of mesoporous metals with asymmetric tetrahedral structures. (ii) One-step simple liquid phase synthesis simplifies the catalyst preparation process and reduces the catalyst preparation cost. (iii) The preparation method is simple, easy to operate, can be prepared in large quantities, and is suitable for large-scale industrial production.
[0015] 2. This invention prepares tetrahedral mesoporous CuPd bimetallic nanocatalysts with unique morphology and functional characteristics for the first time, and applies them to the anode reaction of direct alkaline fuel cells (electrocatalytic ethylene glycol oxidation reaction). Tetrahedral mesoporous CuPd catalysts have three main structural and component advantages: (i) Mesoporous metals can increase the number of catalytic sites, increase unsaturated catalytic sites, improve the utilization rate of precious metal Pd, and reduce the cost of catalytic reactions; (ii) Compared with spherical mesoporous structures, tetrahedral mesoporous structures optimize molecular accessibility, maximize the utilization rate of mesoporous channels, and facilitate the diffusion and transport of reactant molecules, intermediates, and products; (iii) The tetrahedral mesoporous metal framework with good crystallinity is conducive to overcoming Ostwald ripening and improving the stability of the catalytic reaction; (IV) The bimetallic alloy produces a bifunctional effect. Cu not only promotes the electronic oxidation of toxic CO ads In Pd (Pd-CO ads ) and is functionally beneficial to the adsorption of OH groups (Cu-OH ads ) to optimize CO ads Further oxidation of the intermediate. Therefore, the use of this catalyst can not only improve the activity and stability of the electrochemical ethylene glycol oxidation reaction, but also provide a very good research platform for the diffusion dynamics of ethylene glycol molecules in mesoporous metals. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 TEM images of the tetrahedral mesoporous CuPd catalyst (ac) prepared in Example 1 and the spherical mesoporous CuPd catalyst (df) obtained in Comparative Example 1 without adding potassium bromide.
[0017] Figure 2 The tetrahedral mesoporous CuPd catalyst prepared in Example 1 ( th -meso-CuPd) and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd), commercial Pd / C catalyst ( np -Pd) X-ray diffraction pattern.
[0018] Figure 3 The tetrahedral mesoporous CuPd catalyst prepared in Example 1 ( th -meso-CuPd) and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd), commercial Pd / C catalyst ( np Cyclic voltammetry curves of d-Pd.
[0019] Figure 4 The tetrahedral mesoporous CuPd catalyst prepared in Example 1 ( th -meso-CuPd) and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd), commercial Pd / C catalyst ( np Summary of mass and area activities of Pd-Pd.
[0020] Figure 5 The tetrahedral mesoporous CuPd catalyst prepared in Example 1 ( th -meso-CuPd) and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd), commercial Pd / C catalyst ( np Chronoamperometric test diagram of the electrocatalytic ethylene glycol oxidation reaction of Pd-Pd.
[0021] Figure 6 The tetrahedral mesoporous CuPd catalyst prepared in Example 1 ( th -meso-CuPd) and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd), commercial Pd / C catalyst ( np Carbon monoxide stripping voltammetry curve of Pd-Pd.
[0022] Figure 7 The cyclic voltammetry curves of the tetrahedral mesoporous CuPd catalyst prepared in Example 1 at different reaction temperatures (a) and the temperature-mass activity relationship between the tetrahedral mesoporous CuPd catalyst and the commercial Pd / C catalyst (b) are shown. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to these embodiments. Example 1
[0024] 13 mg CTAC was dissolved in 5 mL deionized water at room temperature, and the aqueous solution was gently shaken until dissolved, and 0.8 mL 0.1 mol / L sodium hydroxide aqueous solution was added to adjust the pH to 11.3, and then 0.5 mL 0.08 mol / L potassium bromide aqueous solution, 0.5 mL 0.01 mol / L chloropalladic acid aqueous solution and 0.5 mL 0.01 mol / L copper nitrate aqueous solution were added. The resulting reaction solution was placed in a 50°C oven for reaction for 50 min, and then 0.5 mL 0.3 mol / L L-ascorbic acid aqueous solution was added, and the reaction was continued at 50°C for 2 h; after the reaction was completed, the CTAC was removed by centrifugation with anhydrous ethanol for 6 times, and then dried in a vacuum oven at 50°C to finally obtain a tetrahedral mesoporous CuPd catalyst.
[0025] Comparative Example 1
[0026] In Example 1, potassium bromide was not added as a structure inducing agent, and the remaining steps were exactly the same as in Example 1 to prepare a spherical mesoporous CuPd catalyst.
[0027] Comparative Example 2
[0028] At room temperature, 4 mL of 0.01 mol / L chloropalladic acid aqueous solution and 4 mL of 0.01 mol / L copper nitrate aqueous solution were added to 5.44 mL of 5 mg / mL Vulcan XC-72 aqueous solution. The resulting mixed solution was stirred and dried at room temperature. The powder obtained after drying was poured into 20 mL of 5 mg / mL freshly prepared sodium borohydride aqueous solution. After stirring for 2 h, the product was collected by centrifugation by washing with a mixed solution of ethanol and water, and dried to obtain a particulate CuPd catalyst. Example 2
[0029] In this example, 0.5 mL of 0.08 mol / L sodium bromide aqueous solution was used to replace the potassium bromide aqueous solution in Example 1, and the other steps were the same as those in Example 1 to obtain a tetrahedral mesoporous CuPd catalyst. Example 3
[0030] In this example, 0.5 mL of 0.08 mol / L ammonium bromide aqueous solution was used to replace the potassium bromide aqueous solution in Example 1, and the other steps were the same as those in Example 1 to obtain a tetrahedral mesoporous CuPd catalyst. Example 4
[0031] In this example, 13 mg CTAB was used to replace the CTAC in Example 1, and the other steps were the same as those in Example 1 to obtain a tetrahedral mesoporous CuPd catalyst.
[0032] Figure 1The TEM images of the tetrahedral mesoporous CuPd catalyst prepared in Example 1 and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 are shown. It can be seen that the tetrahedral mesoporous structure has a relatively uniform size and is monodispersed. The side length of the tetrahedron is 80 to 150 nm. The high-magnification TEM image shows that the surface of the tetrahedral mesoporous metal has abundant mesoporous channels, which are branched and radiate from the three edges of the tetrahedron to the center. Figure 1 (c) The simulated structure is consistent. The tetrahedral mesoporous CuPd catalyst prepared in Example 1 was further characterized ( th -meso-CuPd) and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd), commercial Pd / C catalyst ( np -Pd) crystal structure, from Figure 2 From the powder X-ray diffraction (PXRD) patterns, it can be seen that the four groups of samples all show a set of XRD signals corresponding to face-centered cubic (fcc) crystals, which can be attributed to the (111), (200), (220), (311), and (222) crystal planes of fcc crystals. In particular, the alloy components can be observed. th -meso-CuPd, sp -meso-CuPd and np -The diffraction peak of CuPd is compared with np -Pd shifts to a higher angle by 0.76°, indicating th -meso-CuPd, sp -meso-CuPd and np -CuPd all form a CuPd alloy with uniform component distribution. In order to demonstrate the beneficial effects of the present invention, the tetrahedral mesoporous CuPd catalyst ( th -meso-CuPd) and the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd) and commercial Pd / C catalysts ( np -Pd) was used for electrocatalytic oxidation of ethylene glycol, and the current density ( j), which can be used to characterize the electrochemical behavior in this voltage range, where the CV scan rate is 50 mV / s and the scanning voltage range is -0.9 to 0.2 V relative to silver / silver chloride; the constant voltage method can be used to record the chronoamperometric (it) curve under the applied potential; the catalyst catalytic reaction temperature is adjusted by a water bath, and the water bath temperature range is 20 to 35 °C.
[0033] The calculation method of mass activity (MA) is as follows:
[0034]
[0035] Among them, i k is the peak current (A) of the oxidation peak of the tested CV curve; m Pd is the mass of catalyst on the electrode surface normalized to Pd (mg).
[0036] The calculation method of area activity (Specific Activity, SA) is as follows:
[0037]
[0038] Among them, i k is the peak current (A) of the oxidation peak of the tested CV curve; m Pd is the mass of catalyst on the electrode surface normalized to Pd (mg), and ECSA is the electrochemically active area per unit mass of catalyst (m 2 / g).
[0039] Figure 3 The CV curve in sp -meso-CuPd, np -CuPd and np Compared with -Pd, th -meso-CuPd has the highest peak current in a mixed solution of 1 mol / L potassium hydroxide and 1 mol / L ethylene glycol, reaching 7.933 A / mg Pd ,illustrate th -meso-CuPd catalyst has enhanced electrocatalytic activity for ethylene glycol oxidation. Figure 4 The summarized mass activity (MA) and area activity (SA) show that the tetrahedral mesoporous CuPd catalyst exhibits the highest MA and SA, indicating that the tetrahedral mesoporous metal structure has a unique structural advantage over the spherical mesoporous structure, and the mesoporous CuPd ( th -meso-CuPd and sp The MA and SA of 2-meso-CuPd) are significantly better than those of other non-mesoporous structures, demonstrating the importance of reactants in the mesoporous channels for catalytic reactions.
[0040] The electrochemical workstation (CHI660E) was used to carry out the electrocatalytic oxidation reaction of ethylene glycol. The test adopted a three-electrode system. The tetrahedral mesoporous PdCu catalyst ( th -meso-CuPd) and Vulcan XC-72 carbon black were physically loaded in a mass ratio of 1:4, and a catalyst ink with a concentration of 1 mg / mL was prepared using isopropanol: deionized water: naphthol in a volume ratio of 76:19:5 as a solvent. The ink was then drop-coated on a glassy carbon electrode (the electrode diameter of the glassy carbon electrode was 3 mm and the electrode area was 0.07068 cm 2 , the glassy carbon electrode needs to be polished on aluminum oxide powder of different particle sizes before use until the electrode surface is smooth, and the potential difference between the anode and cathode peaks of the cyclic voltammetry curve in potassium ferrocyanide solution is less than 80 mV). The catalyst loading is 0.003 mg. After drying, it is used as a working electrode, a saturated silver / silver chloride electrode is used as a reference electrode, and a 6 mm×6 cm carbon rod electrode is used as a counter electrode. The electrolytic cell uses an ordinary three-electrode electrolytic cell with a mixed solution of 1 mol / L potassium hydroxide and 1 mol / L ethylene glycol as the electrolyte. Before the electrochemical test and during the reduction process, nitrogen with a purity of more than 99.9% needs to be passed to saturation. In the electrochemical test, the reaction potential is -0.9 to 0.2 V relative to the silver / silver chloride electrode, and the reaction temperature is 25°C. Generally speaking, the reaction test temperature is 25°C, but when testing under different reaction temperature conditions, it is necessary to test in a water bath at the required temperature. At the same time, the spherical mesoporous CuPd catalyst prepared in Comparative Example 1 ( sp -meso-CuPd), CuPd granular catalyst prepared in Comparative Example 2 ( np -CuPd), commercial Pd / C catalyst ( np -Pd) for comparative experiments.
[0041] Depend on Figure 5 The chronoamperometric stability test graph shows that at a fixed potential (-0.1 V vs SCE) th -meso-CuPd has the best stability and maintains a higher MA (1.34 A / mg Pd ). Significantly better than other comparison samples: sp -meso-CuPd(0.57 A / mg Pd )、 np - CuPd (0.076 A / mg Pd )、 np -Pd(0.007 A / mg PdBased on the enhanced catalytic activity and stability exhibited by tetrahedral mesoporous metals, the present invention further explores their kinetic and thermodynamic surfaces during the electrocatalytic oxidation of ethylene glycol to understand their enhanced reaction performance.
[0042] The three-electrode test system was further used to test the CO stripping voltammetry curve, using carbon monoxide to simulate the intermediate adsorption during the electrocatalytic oxidation of ethylene glycol. The test was conducted in a 1 mol / L CO-saturated KOH solution, CO was adsorbed for 20 min at open circuit voltage, and the three electrodes were transferred to a new 1 mol / L nitrogen-saturated KOH solution for cyclic voltammetry. Figure 6 The carbon monoxide stripping voltammetry curve shows that compared with the single metal np -Pd, two components th -meso-CuPd, sp -meso-CuPd and np -CuPd shows a lower peak potential, which is 55 mV lower than that of the single metal, proving the existence of bimetallic components, which is conducive to the rapid removal of oxygen-containing intermediates and the further progress of reaction kinetics. Figure 7 The thermodynamic cyclic voltammetry curve and activation energy statistics clearly show that with the increase of temperature, th -meso-CuPd's MA gradually increases ( Figure 7 a), Summary of the relationship between the inverse of temperature and the logarithm of the reaction MA ( Figure 7 b) It can be found that there is a linear relationship between the two physical variables of the two catalysts. According to the Arrhenius equation, it can be calculated that: th -meso-CuPd with np The activation energy of Pd for the electrocatalytic reaction of ethanol oxidation is 19.78 kJ mol -1 and 32.66 kJ mol -1 , th -meso-CuPd significantly reduces the activation energy of the electrocatalytic oxidation reaction of ethylene glycol, thereby facilitating the occurrence of the reaction and improving its catalytic performance.
Claims
1. A method for preparing a tetrahedral mesoporous CuPd catalyst, characterized in that: The cationic surfactant is dissolved in deionized water and the pH is adjusted to 10-12, then a structure inducing agent, chloropalladic acid and copper nitrate are added, the resulting reaction solution is allowed to stand for reaction at 40-60° C. for 30-60 minutes, L-ascorbic acid is added, and the reaction is allowed to stand for reaction at 40-60° C. for 2-3 hours, centrifuged and washed, and vacuum dried to obtain a tetrahedral mesoporous CuPd catalyst; The cationic surfactant is any one or two of cetyltrimethylammonium chloride and cetyltrimethylammonium bromide; the structure inducing agent is any one or more of potassium bromide, sodium bromide and ammonium bromide.
2. The method for preparing the tetrahedral mesoporous CuPd catalyst according to claim 1, characterized in that: The amount of the cationic surfactant added to the deionized water is 1.5-3 mg / mL.
3. The method for preparing the tetrahedral mesoporous CuPd catalyst according to claim 1, characterized in that: The pH is adjusted to 10-12 with 0.1 mol / L sodium hydroxide or potassium hydroxide aqueous solution.
4. The method for preparing the tetrahedral mesoporous CuPd catalyst according to claim 1, characterized in that: The concentration of the structure inducing agent in the reaction solution is 0.005-0.01 mol / L, the concentration of chloropalladic acid is 0.5-1.5 mmol / L, and the concentration of copper nitrate is 0.5-1.5 mmol / L.
5. The method for preparing the tetrahedral mesoporous CuPd catalyst according to claim 1, characterized in that: The added amount of the L-ascorbic acid is 15 to 30 times the total molar amount of chloropalladic acid and copper nitrate.
6. The method for preparing the tetrahedral mesoporous CuPd catalyst according to claim 1, characterized in that: The molar ratio of Pd to Cu in the tetrahedral mesoporous CuPd catalyst is 90:10 to 50:
50.
7. The method for preparing the tetrahedral mesoporous CuPd catalyst according to claim 1, characterized in that: The cationic surfactant was removed by centrifugal washing with ethanol and drying in a vacuum oven at 40-60°C.
Citation Information
Patent Citations
Preparation method and application of core-shell structured Cu@Pd nanometer electrocatalyst for fuel cell
CN108832139A
Preparation method of binary metal platinum-palladium prismatic catalyst and application of binary metal platinum-palladium prismatic catalyst in direct methanol fuel cell
CN113948729A
Metal particle carrying catalyst and its manufacturing method