Spherical-like structured supramolecular low-temperature honeycomb denitrification catalyst and preparation method thereof
By using a supramolecular low-temperature honeycomb denitration catalyst with a spherical structure, using carbon nanotube carriers and hydrothermal synthesis methods, the problems of low catalytic efficiency and weak resistance to alkaline metal poisoning of vanadium-titanium series catalysts at low temperatures have been solved, achieving The improvement of high-efficiency denitrification and anti-poisoning properties is suitable for denitrification treatment in non-electricity industries.
Patent Information
- Application Number
- CN202211486185.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-24
AI Technical Summary
Existing vanadium-titanium catalysts have low catalytic efficiency at low temperatures and weak resistance to alkaline metal poisoning, making them difficult to effectively apply in non-electrical industries.
A supramolecular low-temperature honeycomb denitration catalyst with a spherical structure is used, using carbon nanotubes as a carrier, and combined with a hydrothermal synthesis method to synthesize it in one step. The binder and molding aid form a paste, which is extruded and calcined to obtain a catalyst with high catalytic activity and anti-poisoning properties.
It achieves efficient denitrification at low temperatures, has excellent mechanical properties and resistance to chemical poisoning, and is suitable for denitrification treatment in coal-fired power plants and non-electricity industries, significantly improving the industrial applicability of the catalyst.
Smart Images

Figure CN115920900B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of selective catalytic reduction catalysts, and in particular to a supramolecular low-temperature honeycomb denitration catalyst with a spherical structure and a preparation method thereof. Background Art
[0002] Nitrogen oxides (NO X ) is one of the main pollutants in the atmosphere and is the main cause of environmental problems such as acid rain, ozone layer holes, photochemical smog, etc., affecting the environmental ecosystem and human health. X Pollution source control has very important practical significance.
[0003] Selective catalytic reduction (SCR) denitrification catalyst is the most effective denitrification technology at present, with vanadium-titanium catalyst as the mainstream NO X The treatment methods are becoming mature. However, for non-electric industries such as cement, glass, and steel, vanadium-titanium catalysts cannot achieve very ideal results due to their low low-temperature catalytic efficiency and weak resistance to alkali metals. Therefore, the development of catalysts with low-temperature resistance to alkali metals is a strategic development direction for SCR denitrification to be more widely used in non-electric industries. Summary of the invention
[0004] The object of the present invention is to provide a supramolecular low-temperature honeycomb denitration catalyst with a spherical structure and a preparation method thereof. The supramolecular low-temperature honeycomb denitration catalyst with a spherical structure prepared by the preparation method of the present invention has high low-temperature denitration activity and strong resistance to alkaline metal poisoning.
[0005] One aspect of the present invention provides a method for preparing a spherical-like supramolecular low-temperature honeycomb denitration catalyst, comprising the following steps:
[0006] S1, adding carbon nanotubes to deionized water, adding metal salt solution after ultrasonic dispersion treatment, and stirring to mix;
[0007] S2, adding an alkaline solution to the mixed solution in step S1 and placing the mixed solution in a hydrothermal synthesis reactor to perform a hydrothermal synthesis reaction;
[0008] S3, after the reaction in step S2 is completed, cool to room temperature, pour out the supernatant, centrifuge the remaining suspension with a solvent, and dry to obtain hydrotalcite powder;
[0009] S4, mixing the hydrotalcite powder dried in step S3 with TiO2, adding deionized water, a binder, and a molding aid, mixing evenly to form a paste, and obtaining a supramolecular low-temperature denitration catalyst with a spherical structure after extrusion, drying, and calcination.
[0010] Preferably, the carbon nanotubes described in step S1 include: any one of multi-walled carbon nanotubes and hydroxylated multi-walled carbon nanotubes.
[0011] Preferably, the metal salt solution in step S1 includes: one or more of nickel acetate, ferric nitrate, and manganese acetate; further, the concentration of the metal salt solution is 0.1-1 mol / L.
[0012] Preferably, the mass ratio of the carbon nanotubes to the metal salt solution in step S1 is 1:(200-1000).
[0013] Preferably, the stirring method in step S1 is any one of magnetic stirring and stirring with a stirring paddle.
[0014] In a specific embodiment, step S1 includes: adding carbon nanotubes to deionized water, ultrasonically dispersing for 1 hour, adding 0.1-1 mol / L metal salt solution, and stirring at 60-80° C. for 1 hour.
[0015] Preferably, the alkaline solution in step S2 is one or more of sodium bicarbonate, sodium carbonate and urea.
[0016] Preferably, the mass ratio of the alkaline solution in step S2 to the metal salt solution in step S1 is 1:1; further, the concentration of the alkaline solution is 0.5-3 mol / L.
[0017] In a specific embodiment, step S2 comprises: adding 0.5-3 mol / L alkaline solution to the mixed solution of step S1 and placing the mixed solution in a hydrothermal synthesis reactor for hydrothermal synthesis for 6-24 hours, with the temperature maintained at 90-140°C.
[0018] Preferably, the solvent in step S3 is any one of deionized water, ethanol and ethylene glycol.
[0019] Preferably, the drying temperature in step S3 is 60-90°C.
[0020] In one specific embodiment, step S3 comprises: cooling to room temperature after the reaction in step S2 is completed, pouring out the supernatant, centrifuging the remaining suspension with a solvent, and then drying at 60-90° C. to obtain hydrotalcite powder.
[0021] Preferably, the binder in step S4 is one or more of attapulgite, pottery clay, and sepiolite; and the molding aid is one or more of hydroxymethyl cellulose and hydroxypropyl cellulose.
[0022] Preferably, the paste in step S4 comprises, by mass fraction, 10% hydrotalcite powder, 70% TiO2, 10% deionized water, 5% binder and 5% molding aid.
[0023] In a specific embodiment, step S4 includes: mixing the hydrotalcite powder dried in step S3 with TiO2, adding deionized water, a binder, and a molding aid, mixing evenly to form a paste, extruding, drying, and calcining at 300 to 500°C for 1 to 5 hours to obtain a supramolecular low-temperature honeycomb deNOx catalyst with a spherical structure.
[0024] Another aspect of the present invention provides a supramolecular low-temperature honeycomb denitration catalyst with a spherical structure prepared by any of the preparation methods described above.
[0025] Beneficial effects:
[0026] (1) The spherical-like supramolecular low-temperature honeycomb denitrification catalyst of the present invention is prepared by a one-step hydrothermal synthesis method. The preparation method is simple and efficient, and the catalyst has a high catalytic activity at a relatively low temperature.
[0027] (2) The present invention uses carbon nanotubes as carriers to increase the specific surface area and pore volume of the catalyst carrier, thereby increasing the catalyst's adsorption capacity for harmful elements such as alkaline metals and heavy metals, thereby improving the catalyst's anti-poisoning performance;
[0028] (3) The overall process of the technology of the present invention is simple and low in cost. The prepared spherical-shaped supramolecular low-temperature honeycomb denitrification catalyst has high denitrification performance and excellent mechanical properties and resistance to chemical poisoning. The catalyst has strong industrial applicability and is not only suitable for coal-fired power plants, but also for denitrification control in non-electric industries such as glass and cement. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0030] Figure 1 This is a picture of the appearance of the supramolecular low-temperature honeycomb denitration catalyst with a spherical structure of the present invention. DETAILED DESCRIPTION
[0031] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0032] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] 1. Embodiment 1
[0035] Multi-walled carbon nanotubes were added to deionized water and ultrasonicated for 1 hour, mixed with 0.1 mol / L nickel acetate, ferric nitrate (molar ratio 3:1), and 0.5 mol / L sodium carbonate, stirred at 60°C for 1 hour, and placed in a hydrothermal synthesis kettle for hydrothermal synthesis for 12 hours, with the temperature maintained at 120°C; after the reaction was completed, it was cooled to room temperature, the supernatant was poured out, and the remaining suspension was centrifuged with solvent deionized water, and then dried at 60°C to obtain hydrotalcite powder, mixed with TiO2, deionized water, binder, and molding aid, mixed evenly to form a paste, extruded, dried, and calcined at 300°C for 5 hours to obtain a spherical-shaped supramolecular low-temperature honeycomb denitrification catalyst.
[0036] The mass fraction ratio of the paste ingredients is: 10% of hydrotalcite powder, 70% of TiO2, 10% of deionized water, 5% of binder, and 5% of molding aid.
[0037] 2. Embodiment 2
[0038] Multi-walled carbon nanotubes were added to deionized water and ultrasonicated for 1 hour, mixed with 0.5 mol / L manganese acetate, ferric nitrate (molar ratio 3:1), and 1.5 mol / L sodium bicarbonate, stirred at 60°C for 1 hour, and placed in a hydrothermal synthesis kettle for hydrothermal synthesis for 12 hours, with the temperature maintained at 120°C; after the reaction was completed, it was cooled to room temperature, the supernatant was poured out, and the remaining suspension was centrifuged with solvent deionized water, and then dried at 80°C, mixed with TiO2, deionized water, binder, and molding aid were added, mixed evenly to form a paste, and after extrusion, drying, and calcination at 300°C for 5 hours, a spherical-shaped supramolecular low-temperature honeycomb denitrification catalyst was obtained.
[0039] The mass fraction ratio of the paste ingredients is: 10% of hydrotalcite powder, 70% of TiO2, 10% of deionized water, 5% of binder, and 5% of molding aid.
[0040] 3. Embodiment 3
[0041] Multi-walled carbon nanotubes were added to deionized water and ultrasonicated for 1 hour, mixed with 1 mol / L nickel acetate, ferric nitrate, manganese acetate (molar ratio 3:1:3), 2 mol / L urea, stirred at 80°C for 1 hour, placed in a hydrothermal synthesis kettle for hydrothermal synthesis for 6 hours, and the temperature was maintained at 140°C; after the reaction was completed, it was cooled to room temperature, the supernatant was poured out and the remaining suspension was centrifuged with solvent ethanol, and then dried at 90°C to obtain hydrotalcite powder, mixed with TiO2, added with deionized water, binder, and molding aid, mixed evenly to form a paste, extruded, dried, and calcined at 500°C for 3 hours to obtain a spherical-like supramolecular low-temperature honeycomb denitrification catalyst.
[0042] The mass fraction ratio of the paste ingredients is: 10% of hydrotalcite powder, 70% of TiO2, 10% of deionized water, 5% of binder, and 5% of molding aid.
[0043] 4. Embodiment 4
[0044] Hydroxylated carbon nanotubes were added to deionized water and ultrasonicated for 1 hour, mixed with 1 mol / L nickel acetate, ferric nitrate, manganese acetate (molar ratio 3:1:3), 2.5 mol / L urea, stirred at 80°C for 1 hour, placed in a hydrothermal synthesis kettle for hydrothermal synthesis for 24 hours, and the temperature was maintained at 120°C; after the reaction was completed, it was cooled to room temperature, the supernatant was poured out and the remaining suspension was centrifuged with solvent ethanol, and then dried at 80°C to obtain hydrotalcite powder, mixed with TiO2, deionized water, binder, and molding aid, mixed evenly to form a paste, extruded, dried, and calcined at 400°C for 5 hours to obtain a spherical-like supramolecular low-temperature honeycomb deNOx catalyst.
[0045] The mass fraction ratio of the paste ingredients is: 10% of hydrotalcite powder, 70% of TiO2, 10% of deionized water, 5% of binder, and 5% of molding aid.
[0046] V. Embodiment 5
[0047] The multi-walled carbon nanotubes were added to deionized water and ultrasonicated for 1 hour, and 1 mol / L nickel acetate, ferric nitrate, manganese acetate (molar ratio 3:1:3) and 3 mol / L urea were mixed, stirred at 80°C for 1 hour, and placed in a hydrothermal synthesis reactor for hydrothermal synthesis for 24 hours, and the temperature was maintained at 120°C; after the reaction was completed, it was cooled to room temperature, the supernatant was poured out, and the remaining suspension was centrifuged with solvent ethylene glycol, and then dried at 60°C to obtain hydrotalcite powder, which was mixed with TiO2, deionized water, a binder, and a molding aid were added, mixed evenly to form a paste, and extruded, dried, and calcined at 450°C for 5 hours to obtain a spherical-shaped supramolecular low-temperature honeycomb denitrification catalyst (such as Figure 1 shown).
[0048] The mass fraction ratio of the paste ingredients is: hydrotalcite powder 10%, TiO2 70%, deionized water 10%, binder 5%, molding aid 5%
[0049] VI. Example 6
[0050] Multi-walled carbon nanotubes were added to deionized water and ultrasonicated for 1 hour, mixed with 1 mol / L nickel acetate, ferric nitrate, manganese acetate (molar ratio 3:1:3), 3 mol / L urea, stirred at 80°C for 1 hour, placed in a hydrothermal synthesis kettle for hydrothermal synthesis for 24 hours, and the temperature was maintained at 140°C; after the reaction was completed, it was cooled to room temperature, the supernatant was poured out and the remaining suspension was centrifuged with solvent ethylene glycol, and then dried at 60°C to obtain hydrotalcite powder, mixed with TiO2, added with deionized water, binder, and molding aid, mixed evenly to form a paste, extruded, dried, and calcined at 500°C for 5 hours to obtain a spherical-shaped supramolecular low-temperature honeycomb denitrification catalyst.
[0051] The mass fraction ratio of the paste ingredients is: 10% of hydrotalcite powder, 70% of TiO2, 10% of deionized water, 5% of binder, and 5% of molding aid.
[0052] VII. Comparative Example 1
[0053] Add carbon nanotubes to deionized water and ultrasonicate for 1 hour, place them in a hydrothermal synthesis kettle for hydrothermal synthesis for 6 hours, and maintain the temperature at 90°C; after the reaction is completed, cool to room temperature, pour out the supernatant and centrifuge the remaining suspension with deionized water as a solvent, and then dry at 90°C to obtain hydrotalcite powder, mix it with TiO2, add deionized water, binder, and molding aid, mix well to form a paste, extrude, dry, and calcine at 300°C for 3 hours to obtain a honeycomb denitrification catalyst.
[0054] The mass fraction ratio of the paste ingredients is: 10% of hydrotalcite powder, 70% of TiO2, 10% of deionized water, 5% of binder, and 5% of molding aid.
[0055] 8. Comparative Example 2
[0056] 1 mol / L nickel acetate, ferric nitrate (molar ratio 3:1), and 2 mol / L sodium carbonate were stirred at 80°C for 1 h, placed in a hydrothermal synthesis kettle for hydrothermal synthesis for 24 h, and the temperature was maintained at 120°C; after the reaction was completed, it was cooled to room temperature, the supernatant was poured out, and the remaining suspension was centrifuged with deionized water as a solvent, and then dried at 60-90°C to obtain hydrotalcite powder, which was mixed with TiO2, deionized water, a binder, and a molding aid were added, mixed evenly to form a paste, and extruded, dried, and calcined at 300°C for 5 h to obtain a honeycomb denitrification catalyst.
[0057] The mass fraction ratio of the paste ingredients is: 10% of hydrotalcite powder, 70% of TiO2, 10% of deionized water, 5% of binder, and 5% of molding aid.
[0058] IX. Denitrification performance test
[0059] The denitration performance of the denitration catalysts prepared in the above Examples 1-6 and Comparative Examples 1-2 was tested. Test conditions: test temperature 120°C, 180°C, NH3 concentration 500ppm, NH3 / NO=1, SO2 concentration 200ppm, H2O concentration 3%, reactor space velocity GHSV=60000h -1 .
[0060] The denitration efficiencies of different catalysts are shown in Table 1. The results show that compared with Comparative Examples 1-2, the low-temperature denitration performance of the denitration catalyst prepared in Examples 1-6 is greatly improved.
[0061] Table 1 Denitrification efficiency of different denitrification catalysts
[0062]
[0063]
[0064] 10. Simulated alkaline metal poisoning resistance experiment
[0065] The denitration catalysts prepared in the above-mentioned Examples 1-6 and Comparative Examples 1-2 were subjected to a simulated poisoning experiment, and 1% Na2O was loaded to simulate the alkaline metal poisoning resistance experiment, and the loading was carried out by an impregnation method.
[0066] The test catalyst was loaded with 1% Na2O, and the denitration performance test conditions were the same as the above denitration performance test. The test results are shown in Table 2. The results show that the denitration performance of the denitration catalyst prepared in Comparative Example 1-2 was significantly reduced after simulated poisoning; in contrast, the denitration performance of the denitration catalyst prepared in Example 1-6 was only slightly reduced, demonstrating excellent resistance to alkaline metal poisoning.
[0067] Table 2 Denitrification efficiency of different denitrification catalysts
[0068] 120℃ Denitrification efficiency (%) 180℃ Denitrification efficiency (%) Comparative Example 1 2.3 9.6 Comparative Example 2 18.3 21.2 Example 1 62.2 63.5 Example 2 68.5 73.2 Example 3 81.8 85.4 Example 4 86.8 90.3 Example 5 89.9 93.2 Example 6 83.7 89.1
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. Application of a spherical-like supramolecular low-temperature honeycomb denitration catalyst in a denitration reaction, characterized in that: The preparation method of the catalyst comprises the following steps: S1. Add carbon nanotubes to deionized water, add metal salt solution after ultrasonic dispersion treatment, and stir to mix; the metal salt solution includes nickel acetate, ferric nitrate and manganese acetate; the carbon nanotubes are hydroxylated multi-walled carbon nanotubes; the mass ratio of the carbon nanotubes to the metal salt solution is 1:(200-1000); S2, adding an alkaline solution to the mixed solution in step S1 and placing the mixture in a hydrothermal synthesis reactor for hydrothermal synthesis reaction for 12-24 hours, with the temperature maintained at 90-140° C.; the alkaline solution is one or more of sodium bicarbonate, sodium carbonate, and urea; S3, after the reaction in step S2 is completed, cool to room temperature, pour out the supernatant, centrifuge the remaining suspension with a solvent, and dry to obtain hydrotalcite powder; S4, mixing the hydrotalcite powder dried in step S3 with TiO2, adding deionized water, a binder, and a molding aid, mixing evenly to form a paste, and obtaining a supramolecular low-temperature denitration catalyst with a spherical structure after extrusion, drying, and calcination.
2. The use according to claim 1, characterized in that: The mass ratio of the alkaline solution in step S2 to the metal salt solution in step S1 is 1:
1.
3. The use according to claim 1, characterized in that: The solvent described in step S3 is any one of deionized water, ethanol, and ethylene glycol.
4. The use according to claim 1, characterized in that: The binder described in step S4 is one or more of attapulgite, pottery clay, and sepiolite; the molding aid is one or more of hydroxymethyl cellulose and hydroxypropyl cellulose.
5. The use according to claim 1, characterized in that: The paste described in step S4 includes, by mass fraction, 10% hydrotalcite powder, 70% TiO2, 10% deionized water, 5% binder and 5% molding aid.