A TiAl-based composite material with a two-stage enhanced three-dimensional network structure and a preparation method thereof

Through high-energy ball milling and powder metallurgy technology, TiAl-based composite materials with two-level reinforced three-dimensional network structures are prepared, which solves the forming difficulties and insufficient plasticity of TiAl-based composite materials, and significantly improves their high-temperature strength and ductility.

CN115921874BActive Publication Date: 2024-10-22CHANGCHUN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211406194.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-10
Publication Date
2024-10-22
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

TiAl-based composite materials are difficult to process and form due to their inherent brittleness, and ordinary methods increase strength while decreasing plasticity, and cannot effectively balance strength and plasticity.

Method used

High-energy ball milling is used to alloy the titanium-aluminum matrix, and is mixed and sintered with titanium pre-alloyed powder to prepare a TiAl-based composite material with a two-level reinforced three-dimensional network structure. The interface bonding strength and density of the material are improved through refinement and mechanical alloying. .

Benefits of technology

It significantly improves the high-temperature ductility and high-temperature plasticity of TiAl-based composite materials, solves the problems of difficult cold forming and poor high-temperature ductility, and achieves a balanced improvement in strength and plasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115921874B_ABST
    Figure CN115921874B_ABST
Patent Text Reader

Abstract

The present invention discloses a TiAl-based composite material with a two-stage enhanced three-dimensional network structure and a preparation method thereof, comprising the following steps: (1) mixing titanium powder, aluminum powder, niobium powder and chromium powder in a molar ratio of 41.5-50.5:43-47:5-9:1.5-2.5 and ball milling to obtain mechanical alloying powder; (2) uniformly mixing the mechanical alloying powder prepared in step (1) with titanium pre-alloyed powder in a mass ratio of 44-47:3-6 to obtain a mixed powder; (3) vacuum hot pressing and sintering the mixed powder to obtain the TiAl-based composite material. The above-mentioned preparation method is simple, and the raw materials are easily available and low in cost. The prepared composite material matrix has fine microstructure, uniform distribution of alloy particles, and no defects such as voids and cracks; in addition, the two-stage reinforcement effect of the α2-Ti3Al phase reinforcing the matrix γ-TiAl phase and the close combination of the titanium alloy powder particles and the matrix titanium aluminum-based alloy effectively improves the high-temperature strength and plasticity of the titanium aluminum-based composite material, so that it has good application prospects in the field of high-temperature alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium-aluminum-based composite material preparation, and in particular to a TiAl-based composite material with a two-stage enhanced three-dimensional network structure and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of aerospace, the requirements for the performance of aerospace parts have also increased accordingly, especially the ductility. γ-TiAl-based composite materials have the advantages of good high-temperature performance and high strength. As high-temperature structural materials, they have good application prospects in the aerospace and automotive industries. However, due to the inherent intrinsic brittleness of ordinary TiAl-based alloys, it is difficult to process them by conventional methods. This shortcoming seriously restricts their widespread application.

[0003] At present, in order to further improve the performance of TiAl-based composite materials, ceramic particles with small particle size and high hardness are usually introduced into the matrix, such as TiB 2 、Ti 2 AlC、Ti 2 AlN and Ti 5 Si 3 Although the introduction of these particles can improve the strength of TiAl-based composites, the plasticity is reduced. For example, Shu et al. introduced B into the TiAl matrix by in-situ reaction sintering. 4 TiB 2 -Ti 2 AlC / TiAl composite material, in which nano-scale TiB is generated 2 and Ti 2 AlC reinforced particles effectively improve the strength of the composite material, but the plasticity is poor. (Shu S,Qiu F,Lin Y,et al.Effect ofB4C size on the fabrication and compression properties of in situ TiB 2 -Ti 2 AlC / TiAl composites[J].Journal of Alloys&Compounds,2013,551:88-91.) In recent years, researchers have proposed to prepare composite materials with three-dimensional network structures to balance strength and plasticity. However, current research is mostly to build a reinforced structure with fine particles as a rigid skeleton in Ti-based, Al-based or TiAl-based composite materials. These research results show that the three-dimensional network structure can improve strength, but the improvement effect on plasticity is not obvious. Therefore, there is an urgent need for a TiAl-based composite material that can effectively balance strength and plasticity. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a TiAl-based composite material with a two-stage reinforced three-dimensional network structure and a preparation method thereof, which can effectively balance the strength and plasticity of the composite material. The present invention uses each element powder as a raw material to achieve alloying of the titanium aluminum matrix through high-energy ball milling, and then mixes and sintered with titanium pre-alloyed powder to prepare a titanium aluminum-based composite material with a new structure. The TiAl-based composite material prepared by the above method has improved high-temperature strength and greatly improved high-temperature ductility of the composite material, thereby effectively solving the problems of difficult cold processing and poor high-temperature ductility of the TiAl-based composite material.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A first aspect of the present invention provides a method for preparing a TiAl-based composite material, comprising the following steps:

[0007] (1) mixing titanium powder, aluminum powder, niobium powder and chromium powder in a molar ratio of 41.5-50.5:43-47:5-9:1.5-2.5 and ball milling to obtain a mechanical alloying powder;

[0008] (2) uniformly mixing the mechanical alloying powder prepared in step (1) with titanium pre-alloy powder in a mass ratio of 44-47:3-6 to obtain a mixed powder; the titanium pre-alloy powder comprises one or more of α single-phase titanium, β single-phase titanium, and α+β dual-phase titanium;

[0009] (3) The mixed powder is subjected to vacuum hot pressing sintering to obtain the TiAl-based composite material.

[0010] Furthermore, in step (1), the mass ratio of the titanium powder, aluminum powder, niobium powder and chromium powder is 42-50:43-47:5-9:2, for example, 46:45:7:2.

[0011] Furthermore, in step (1), the maximum particle size of the titanium powder is ≤40 μm, the maximum particle size of the aluminum powder is ≤120 μm, the maximum particle size of the niobium powder is ≤50 μm, and the maximum particle size of the chromium powder is ≤100 μm.

[0012] Furthermore, in step (1), each element powder and stainless steel balls are added into a ball mill for high-energy ball milling and mechanical alloying.

[0013] Furthermore, in step (1), the ball-to-material ratio of the ball mill is 10 to 15:1.

[0014] During high-energy ball milling, the ball-to-material ratio needs to be controlled to achieve the effect of uniform refinement and mechanical alloying. If the ball-to-material ratio is too small, the powder refinement effect is poor and the mechanical alloying effect is weakened. If the ball-to-material ratio is too large, too many steel balls will lead to uneven mechanical alloying. Therefore, the ball-to-material ratio needs to be controlled within an appropriate range, such as 10 to 15:1.

[0015] Furthermore, in step (1), the rotation speed of the ball mill is 500-550 rpm, and the ball milling time is 30-40 h.

[0016] Furthermore, in step (1), the maximum particle size of the mechanically alloyed powder is ≤1 μm.

[0017] The present invention uses element powder with micron particle size as raw material, performs mechanical alloying under high-energy ball milling, and obtains nano-scale alloyed powder, which can better control the phase composition of the matrix, thereby improving the interface composition and interface bonding strength of the composite material, and the nano-scale alloy powder can effectively reduce the formation of pores, thereby improving the density of the alloy material.

[0018] Furthermore, in step (2), the maximum particle size of the titanium pre-alloy powder is ≤40 μm.

[0019] Furthermore, in step (2), the titanium pre-alloy powder is Ti-6Al-4V.

[0020] Furthermore, in step (2), the mechanical alloying powder and the titanium pre-alloyed powder are placed in a powder mixer for mixing; the ball-to-material ratio of the mixed powder is 2 to 4:1, the rotation speed is 150 to 200 rpm, and the time is 2 to 4 hours.

[0021] Furthermore, in step (3), the specific operation of the vacuum hot pressing sintering is: heating to 1150-1250° C. at a heating rate of 6-10° C. / min, and keeping the temperature and pressure for 40-90 minutes.

[0022] Furthermore, the vacuum hot pressing sintering pressure is 30-50 MPa.

[0023] Furthermore, after vacuum hot pressing sintering, the material is naturally cooled to room temperature in the furnace to obtain the TiAl-based composite material.

[0024] At present, TiAl-based composite materials prepared by traditional preparation methods such as forging and casting are prone to defects such as macrosegregation, uneven structure, coarse grains, insufficient density, etc. The present invention uses powder metallurgy technology to prepare TiAl-based composite materials. The method is simple to operate and can better control the phase composition and grain size of the composite material. After forming, the performance can be further improved by mechanical processing methods such as rolling.

[0025] The second aspect of the present invention provides a TiAl-based composite material prepared by the preparation method described in the first aspect.

[0026] Furthermore, the TiAl-based composite material has a two-level reinforced three-dimensional network structure.

[0027] Beneficial effects of the present invention:

[0028] 1. The present invention uses mechanical ball milling to prepare a nano-scale titanium-aluminum-based alloy with a fine-grained structure, and introduces micron-scale titanium pre-alloy powder into the titanium-aluminum-based alloy through powder metallurgy to prepare a TiAl-based composite material. 2 -Ti 3 The Al phase strengthens the matrix γ-TiAl phase to form a primary reinforcement structure, while the micron-sized titanium alloy powder particles are tightly combined with the matrix titanium-aluminum-based alloy and have a clear transition interface. The phase composition of the transition interface is γ+α 2 →α 2 →α 2 +α→α, forming a two-level reinforcement structure; under the synergistic effect of the above two-level reinforcement structure, the TiAl-based composite material has higher interface strength, better stability and more excellent mechanical properties than ordinary titanium aluminum alloy materials.

[0029] 2. The strengthening and toughening mechanism of the TiAl-based composite material prepared by the present invention is as follows: when the TiAl-based composite material with a two-stage reinforced three-dimensional network structure is deformed, the titanium alloy particles first undergo plastic deformation due to their relatively soft characteristics. At the same time, the TiAl matrix has not reached a yield state and exhibits elastic deformation in accordance with Hooke's law. At this time, dislocations, twins, etc. generated by the deformation accumulate at the interface, thereby obtaining a work hardening effect, which makes the yield strength of the composite material higher than that of the unreinforced TiAl-based alloy; and in subsequent deformation, the titanium alloy particles and the TiAl matrix undergo plastic deformation at the same time. Due to the existence of the interface, the composite material effectively inhibits crack propagation, thereby improving the strength and plasticity of the material at the same time.

[0030] 3. The present invention provides a method for preparing a TiAl-based composite material. The method is simple to operate, the raw materials are readily available, and the cost is low. The prepared composite material has a fine matrix microstructure, uniform distribution of alloy particles, and no defects such as voids and cracks. The composite material has high density and stable performance. Compared with titanium-aluminum-based alloys not doped with titanium pre-alloyed powder, the high-temperature strength of the TiAl-based composite material prepared by the present invention is improved, and the high-temperature plasticity is significantly improved. The tensile plasticity at 900°C is greater than 45%, which is conducive to hot working and forming, and has good application prospects in the field of high-temperature alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1X-ray diffraction patterns of the TiAl-based composite material prepared in Example 1 and the titanium-aluminum-based alloy prepared in Comparative Example 1;

[0032] Figure 2 This is a scanning electron microscope image of the microstructure of the TiAl-based composite material prepared in Example 1, with a scale of 100 μm;

[0033] Figure 3 This is a scanning electron microscope image of the microstructure of the TiAl-based composite material prepared in Example 1, with a scale of 2 μm;

[0034] Figure 4 This is a scanning electron microscope image of the microstructure of the TiAl-based composite material prepared in Example 1, with a scale of 10 μm;

[0035] Figure 5 This is the electron microscope energy spectrum of the TiAl-based composite material prepared in Example 1. DETAILED DESCRIPTION

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0038] Example 1

[0039] The present embodiment relates to the preparation of a TiAl-based composite material, using the following raw materials: titanium powder with a maximum particle size of ≤40 μm, aluminum powder with a maximum particle size of ≤120 μm, niobium powder with a maximum particle size of ≤50 μm, chromium powder with a maximum particle size of ≤100 μm, and titanium pre-alloyed Ti-6Al-4V powder (brand TC4) with a maximum particle size of ≤40 μm.

[0040] The specific preparation process is as follows:

[0041] (1) titanium powder, aluminum powder, niobium powder and chromium powder were loaded into a vacuum ball mill in a molar ratio of 46:45:7:2 (50 g in total), and 500 g of stainless steel balls were added for high-energy ball milling at a speed of 550 r / min for 40 h until the maximum particle size of the powder was ≤1 μm, thereby obtaining a mechanical alloying powder;

[0042] (2) 47 g of the mechanical alloying powder prepared in step (1) and 3 g of titanium pre-alloyed Ti-6Al-4V powder were placed in a powder mixer, the powder mixing speed was set to 150 r / min, the powder mixing time was set to 2 h, and they were fully and evenly mixed;

[0043] (3) The powder mixed evenly in step (2) is loaded into a graphite mold for vacuum hot pressing sintering at a pressure of 30 MPa, a temperature of 1200° C., and a sintering time of 60 min. The powder is cooled to room temperature in the furnace to obtain a TiAl-based composite material (6wt.% TC4 / Ti-45Al-7Nb-2Cr).

[0044] The TiAl-based composite material prepared in this example was characterized by X-ray diffraction and scanning electron microscopy.

[0045] X-ray diffraction characterization results are shown in Figure 1 As shown in the XRD diagram of the sample 6wt.%TC4 / Ti-45Al-7Nb-2Cr, it can be observed that the phases belong to γ-TiAl, α 2 -Ti 3 The diffraction peaks of Al phase, α-Ti phase and β-Ti phase indicate that there are γ-TiAl phase, α-Ti phase and β-Ti phase in the prepared TiAl-based composite material. 2 -Ti 3 Al phase, α-Ti phase and β-Ti phase.

[0046] The scanning electron microscopy results are shown in Figures 2 to 4 As shown, from Figure 2 A gray titanium-aluminum-based alloy matrix and round light black titanium alloy particles can be observed, and the black ring between the two is the interface area. Figure 3 for Figure 2 A local enlarged view of the 2 -Ti 3 The Al phase is evenly distributed in the matrix γ-TiAl phase, forming a three-dimensional network structure.

[0047] Figure 4 for Figure 2 Another partial enlarged picture shows that the micron-sized titanium alloy powder particles are tightly combined with the matrix titanium aluminum alloy and have a clear transition interface. The composition of the transition interface is analyzed using electron microscope energy spectrum and phase diagram. The electron microscope energy spectrum characterization results are shown in Figure 5 As shown in the figure, the Al element in the matrix (line ② in the figure) diffuses into the titanium alloy, and the Ti (line ① in the figure) and V (line ③ in the figure) elements in the titanium alloy diffuse into the matrix, forming a gradient change in the structure at the interface. The phase composition of the transition interface from the matrix to the titanium alloy powder particles is γ+α 2 →α 2 →α2 +α→α, this gradually progressive interface phase composition is beneficial to improving the interface bonding strength between titanium alloy powder particles and the matrix titanium aluminum based alloy.

[0048] Example 2

[0049] The present embodiment relates to the preparation of a TiAl-based composite material, using the following raw materials: titanium powder with a maximum particle size of ≤40 μm, aluminum powder with a maximum particle size of ≤120 μm, niobium powder with a maximum particle size of ≤50 μm, chromium powder with a maximum particle size of ≤100 μm, and titanium pre-alloyed Ti-6Al-4V powder (brand TC4) with a maximum particle size of ≤40 μm.

[0050] The specific preparation process is as follows:

[0051] (1) titanium powder, aluminum powder, niobium powder and chromium powder were loaded into a vacuum ball mill in a molar ratio of 46:45:7:2 (50 g in total), and 500 g of stainless steel balls were added for high-energy ball milling at a speed of 550 r / min for 40 h until the powder particle size was ≤1 μm, thereby obtaining a mechanical alloying powder;

[0052] (2) 46 g of the mechanical alloying powder prepared in step (1) and 4 g of titanium pre-alloyed Ti-6Al-4V powder were placed in a powder mixer, the powder mixing speed was set to 150 r / min, the powder mixing time was set to 2 h, and they were fully and evenly mixed;

[0053] (3) The powder mixed evenly in step (2) is loaded into a graphite mold for vacuum hot pressing sintering at a pressure of 30 MPa, a temperature of 1200° C., and a sintering time of 60 min. The powder is cooled to room temperature in the furnace to obtain a TiAl-based composite material (8 wt.% TC4 / Ti-45Al-7Nb-2Cr).

[0054] Example 3

[0055] The present embodiment relates to the preparation of a TiAl-based composite material, using the following raw materials: titanium powder with a maximum particle size of ≤40 μm, aluminum powder with a maximum particle size of ≤120 μm, niobium powder with a maximum particle size of ≤50 μm, chromium powder with a maximum particle size of ≤100 μm, and titanium pre-alloyed Ti-6Al-4V powder (brand TC4) with a maximum particle size of ≤40 μm.

[0056] The specific preparation process is as follows:

[0057] (1) titanium powder, aluminum powder, niobium powder and chromium powder were loaded into a vacuum ball mill in a molar ratio of 46:45:7:2 (50 g in total), and 500 g of stainless steel balls were added for high-energy ball milling at a speed of 550 r / min for 40 h until the powder particle size was ≤1 μm, thereby obtaining a mechanical alloying powder;

[0058] (2) 45 g of the mechanical alloying powder prepared in step (1) and 5 g of titanium pre-alloyed Ti-6Al-4V powder were placed in a powder mixer, the powder mixing speed was set to 150 r / min, the powder mixing time was set to 2 h, and they were fully and evenly mixed;

[0059] (3) The powder mixed evenly in step (2) is loaded into a graphite mold for vacuum hot pressing sintering at a pressure of 30 MPa, a temperature of 1200° C., and a sintering time of 60 min. The powder is cooled to room temperature in the furnace to obtain a TiAl-based composite material (10 wt.% TC4 / Ti-45Al-7Nb-2Cr).

[0060] Example 4

[0061] The present embodiment relates to the preparation of a TiAl-based composite material, using the following raw materials: titanium powder with a maximum particle size of ≤40 μm, aluminum powder with a maximum particle size of ≤120 μm, niobium powder with a maximum particle size of ≤50 μm, chromium powder with a maximum particle size of ≤100 μm, and titanium pre-alloyed Ti-6Al-4V powder (brand TC4) with a maximum particle size of ≤40 μm.

[0062] The specific preparation process is as follows:

[0063] (1) titanium powder, aluminum powder, niobium powder and chromium powder were loaded into a vacuum ball mill in a molar ratio of 46:45:7:2 (50 g in total), and 500 g of stainless steel balls were added for high-energy ball milling at a speed of 550 r / min for 40 h until the powder particle size was ≤1 μm, thereby obtaining a mechanical alloying powder;

[0064] (2) 44 g of the mechanically alloyed powder prepared in step (1) and 6 g of titanium pre-alloyed Ti-6Al-4V powder were placed in a powder mixer, the mixing speed was set to 150 r / min, the mixing time was set to 2 h, and the mixture was fully and evenly mixed;

[0065] (3) The powder mixed evenly in step (2) is loaded into a graphite mold for vacuum hot pressing sintering at a pressure of 30 MPa, a temperature of 1200° C., and a sintering time of 60 min. The powder is cooled to room temperature in the furnace to obtain a TiAl-based composite material (12 wt.% TC4 / Ti-45Al-7Nb-2Cr).

[0066] In the above-mentioned Examples 1 to 4, only the mass ratio of the mechanical alloying powder to the titanium pre-alloyed powder was changed to prepare the corresponding TiAl-based composite materials.

[0067] Comparative Example 1

[0068] This comparative example relates to the preparation of a titanium-aluminum-based alloy, using the following raw materials: titanium powder with a maximum particle size of ≤40 μm, aluminum powder with a maximum particle size of ≤120 μm, niobium powder with a maximum particle size of ≤50 μm, and chromium powder with a maximum particle size of ≤100 μm.

[0069] The specific preparation process is as follows:

[0070] (1) titanium powder, aluminum powder, niobium powder and chromium powder were loaded into a vacuum ball mill in a molar ratio of 46:45:7:2 (50 g in total), and 500 g of stainless steel balls were added for high-energy ball milling at a speed of 550 r / min for 40 h until the powder particle size was ≤1 μm, thereby obtaining a mechanical alloying powder;

[0071] (2) 50 g of alloyed Ti-45Al-7Nb-2Cr alloy powder was loaded into a graphite mold for vacuum hot pressing sintering at a pressure of 30 MPa, a temperature of 1200°C, and a sintering time of 60 min. The powder was cooled to room temperature to obtain a titanium-aluminum-based alloy (Ti-45Al-7Nb-2Cr).

[0072] The titanium-aluminum alloy prepared in this comparative example was characterized by X-ray diffraction. Figure 1 As shown in the XRD diagram of the sample Ti-45Al-7Nb-2Cr, it can be observed that the phases belong to γ-TiAl phase, α 2 -Ti 3 The diffraction peak of Al phase indicates that there are γ-TiAl phase, α-TiAl phase and 2 -Ti 3 Al phase.

[0073] Comparative Example 2

[0074] The present embodiment relates to the preparation of a TiAl-based composite material, using the following raw materials: titanium powder with a maximum particle size of ≤40 μm, aluminum powder with a maximum particle size of ≤120 μm, niobium powder with a maximum particle size of ≤50 μm, chromium powder with a maximum particle size of ≤100 μm, and titanium pre-alloyed Ti-6Al-4V powder (brand TC4) with a maximum particle size of ≤40 μm.

[0075] The specific preparation process is as follows:

[0076] (1) titanium powder, aluminum powder, niobium powder and chromium powder were loaded into a vacuum ball mill in a molar ratio of 46:45:7:2 (50 g in total), and 500 g of stainless steel balls were added for high-energy ball milling at a speed of 550 r / min for 40 h until the powder particle size was ≤1 μm, thereby obtaining a mechanical alloying powder;

[0077] (2) 48 g of the mechanical alloying powder prepared in step (1) and 2 g of titanium pre-alloyed Ti-6Al-4V powder were placed in a powder mixer, the mixing speed was set to 150 r / min, the mixing time was set to 2 h, and the mixture was fully and evenly mixed;

[0078] (3) The powder mixed evenly in step (2) is loaded into a graphite mold for vacuum hot pressing sintering at a pressure of 30 MPa, a temperature of 1200° C., and a sintering time of 60 min. The powder is cooled to room temperature in the furnace to obtain a TiAl-based composite material (4 wt.% TC4 / Ti-45Al-7Nb-2Cr).

[0079] Performance Testing

[0080] The TiAl-based composite materials prepared in the above Examples 1 to 4 and the titanium-aluminum-based composite materials prepared in Comparative Examples 1 and 2 were made into tensile specimens, and the tensile properties of each specimen were tested. The test method is as follows:

[0081] The polished tensile specimens were placed in a high-temperature tensile testing machine and the tensile temperature was set at 900 °C and the tensile rate was set at 1 × 10 -4 s -1 After the temperature rises to 900℃, keep it warm for 10 minutes and start the tensile test. The high temperature tensile test method of metal materials refers to the national standard GB4338-2006.

[0082] The test results are shown in Table 1:

[0083] Table 1 Tensile performance test data of different samples

[0084] Tensile specimen 900℃ tensile strength / MPa 900℃ tensile plasticity / % Example 1 260 46.8 Example 2 259 47.1 Example 3 258 47.5 Example 4 257 47.9 Comparative Example 1 250 7.2 Comparative Example 2 244 37

[0085] As can be seen from Table 1, Examples 1 to 4 prepare TiAl-based composite materials by introducing an appropriate amount of micron-grade titanium pre-alloyed powder into a titanium-aluminum-based alloy by powder metallurgy. Compared with the unreinforced titanium-aluminum-based alloy, the high-temperature tensile plasticity is significantly improved, and the 900°C tensile plasticity is more than 46%. At the same time, the high-temperature tensile strength is also optimized to a certain extent; however, the amount of micron-grade titanium pre-alloyed powder added is too small, for example, the 4wt.% TC4 / Ti-45Al-7Nb-2Cr prepared in Comparative Example 2, its high-temperature tensile plasticity is significantly improved, but the high-temperature tensile strength is lower than that of the unreinforced titanium-aluminum-based alloy prepared in Comparative Example 1.

[0086] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a TiAl-based composite material, characterized in that: The following steps are involved: (1) mixing titanium powder, aluminum powder, niobium powder and chromium powder in a molar ratio of 41.5-50.5:43-47:5-9:1.5-2.5 and ball milling to obtain a mechanical alloying powder; the maximum particle size of the titanium powder is ≤40 μm, the maximum particle size of the aluminum powder is ≤120 μm, the maximum particle size of the niobium powder is ≤50 μm, the maximum particle size of the chromium powder is ≤100 μm, and the maximum particle size of the mechanical alloying powder is ≤1 μm; (2) mixing the mechanical alloying powder prepared in step (1) with titanium pre-alloy powder in a mass ratio of 44-47:3-6 to obtain a mixed powder; the titanium pre-alloy powder comprises one or more of α single-phase titanium, β single-phase titanium, and α+β dual-phase titanium; and the maximum particle size of the titanium pre-alloy powder is ≤40 μm; (3) The mixed powder is subjected to vacuum hot pressing sintering to obtain the TiAl-based composite material.

2. The preparation method according to claim 1, characterized in that: In step (1), the ball-to-material ratio of the ball mill is 10 to 15:1; the rotation speed of the ball mill is 500 to 550 rpm, and the ball milling time is 30 to 40 hours.

3. The preparation method according to claim 1, characterized in that: In step (2), the titanium pre-alloy powder is Ti-6Al-4V.

4. The preparation method according to claim 1, characterized in that: In step (2), the mechanical alloying powder and the titanium pre-alloyed powder are placed in a powder mixer for mixing; the ball-to-material ratio of the mixed powder is 2 to 4:1, the rotation speed is 150 to 200 rpm, and the time is 2 to 4 hours.

5. The preparation method according to claim 1, characterized in that: In step (3), the specific operation of the vacuum hot pressing sintering is: heating to 1150-1250°C at a heating rate of 6-10°C / min, and keeping the temperature and pressure for 40-90 minutes.

6. The preparation method according to claim 5, characterized in that: The pressure of the vacuum hot pressing sintering is 30-50 MPa.

7. A TiAl-based composite material prepared by the preparation method according to any one of claims 1 to 6.