Fireproof insulation board with ground glass added and preparation method thereof
By adding ground glass fiber and water-soluble resin glue to glass fiber non-textile materials, the fire-resistant insulation board is made by needle-punching process, which solves the problem of insufficient thermal conductivity and flame retardant performance of existing materials and achieves a lower thermal conductivity coefficient and higher flame retardant properties, suitable for exterior wall insulation of high-rise buildings.
Patent Information
- Application Number
- CN202211475393.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-23
AI Technical Summary
Existing building insulation materials have shortcomings in thermal conductivity, flame retardant properties, construction convenience and bonding strength, especially inorganic insulation materials have high thermal conductivity, easy layering, low tensile and compressive strength, and water absorption. and insufficient bonding strength.
Add grated glass fiber to the non-textile material and use water-soluble resin glue to make a fire-resistant insulation board through needle puncture process to reduce the internal pore size of the material, improve convection heat transfer obstacles, enhance tensile and compression performance, and pass Needle-pin hooking and water-soluble resin bonding enhance vertical tensile strength.
It significantly reduces the thermal conductivity, improves the flame retardant performance and construction convenience of insulation materials, ensures the stable insulation performance of the product and the safe application of high-rise buildings.
Smart Images

Figure CN115925318B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to thermal insulation material technology and application fields, and in particular to a fireproof thermal insulation board with ground glass added thereto and a preparation method thereof. Background Art
[0002] At present, in the building insulation industry, external wall insulation mainly adopts two types of insulation materials: inorganic insulation materials and organic insulation materials. Organic insulation materials represented by polystyrene boards have the advantages of low density, low thermal conductivity, good dimensional stability, high vertical tensile strength and high compressive strength, but due to the limitations of the properties of organic insulation materials themselves, they often do not have flame retardant properties. Inorganic insulation materials represented by rock wool have good flame retardant properties, but have disadvantages such as high thermal conductivity, easy stratification, low vertical tensile strength and low compressive strength, and have problems such as high water absorption and low bonding strength between surface layers during long-term use. There are safety hazards such as wall shedding during use.
[0003] The public patent "A new type of insulation board and its production process" (application number: CN202010566915.4) provides a new type of insulation board containing only glass fiber and phenolic resin. Through specific material selection and ratio, the mechanical properties and thermal insulation properties are guaranteed. It is said that the thermal conductivity of the obtained insulation board can reach 0.028~0.035W / (m·K). Its preparation method includes feeding, unpacking, loosening, combing, laying, needling, cutting, spraying, extruding glue, and curing molding processes. However, the preparation process involves a needling process. Ordinary glass fiber needle-punched hook-linked non-woven insulation materials have many holes between fibers due to the needling and fiber overlapping during the production process, which leads to a high convective heat transfer rate during heat conduction, thereby limiting the improvement of the thermal conductivity of the insulation material and causing unstable thermal conductivity. Summary of the invention
[0004] In order to solve the problems existing in the above-mentioned insulation board, the present invention proposes a fireproof insulation board with added ground glass and a preparation method thereof. By adding ground glass fiber inside the glass fiber non-woven material, the number and size of pores inside the material can be significantly reduced, the convective heat transfer barrier can be increased, and the thermal conductivity coefficient can be reduced. Since the insulation material is made of non-combustible glass fiber through a needle punching process and water-soluble resin glue is sprayed during the production process, the vertical tensile and compression properties of the insulation material are improved. At the same time, the product is easy to construct and has strong bonding with mortar, and can be widely used in building exterior walls and pipeline insulation. The technical solution of the present invention is as follows:
[0005] As a first aspect of the present invention, there is provided a fireproof insulation board with added ground glass, comprising the following components: ground glass fibers in the form of ground glass, glass fibers in the form of glass fiber mat, and water-soluble resin glue, wherein the ground glass fibers are dispersed in the glass fiber mat and the water-soluble resin glue.
[0006] Preferably, the content of the ground glass fiber is 0.5-15%, preferably 1%-15%, more preferably 1%-5%; the content of the glass fiber in the glass fiber mat is 80%-97%, and the content of the water-soluble resin glue is 2.5-10%, preferably 6%.
[0007] Preferably, the milled glass fiber component is selected from one or more of alkali-free glass fiber, medium-alkali glass fiber, high-alkali glass fiber and alkali-resistant glass fiber; the length is 30μm to 150μm, the diameter is 3μm to 80μm, and the length is further preferably 30μm to 100μm, and the diameter is 3μm to 30μm.
[0008] Preferably, the glass fiber component in the glass fiber mat is selected from E glass fiber, including starch-type, water-drawn type or thermoplastic short-cut products; the length is 50mm to 120mm, and the diameter is 5μm to 30μm.
[0009] Furthermore, the glass fibers in the glass fiber mat are preferably a combination of FED9-70 and FED6-70, wherein the FED9-70 glass fibers are 50 mm to 100 mm in length and 8 μm to 10 μm in diameter, and the FED6-70 glass fibers are 50 mm to 100 mm in length and 5 μm to 7 μm in diameter. The more preferred ratio is FED9-70:FED6-70=90:10.
[0010] Furthermore, the milled glass fiber is made of E glass milled fiber with a length of 50 μm and a diameter of 8 μm.
[0011] Preferably, the thickness of the fireproof insulation board product with added ground glass is between 4 mm and 150 mm.
[0012] As a second aspect of the present invention, there is provided a method for preparing the fireproof heat-insulating board with added ground glass, comprising the following steps:
[0013] Step 1, loading;
[0014] Step 2, fluffing treatment, rough opening and fine opening treatment are performed in the opening machine;
[0015] Step 3: finishing the net, and processing it in a finishing machine to obtain a fiber net, the single-layer net weight of the fiber net is 80-140g / m 2 ;
[0016] Step 4, applying glue and laying the web, spraying the water-soluble resin glue added with the ground glass fiber onto the fiber web obtained in step 3, and laying the glue-sprayed fiber web in multiple layers continuously to form a glue-sprayed fiber web layer;
[0017] Step 5, needle-punching into felt, needle-punching the spray-bonded fiber mesh layer obtained in step 4, including pre-puncturing from top to bottom and barbing from bottom to top, to obtain a glass fiber felt;
[0018] Step 6, curing, curing the glass fiber mat obtained in step 5 into shape.
[0019] Furthermore, in step 4, the ground glass fibers are first added to the water-soluble resin glue and stirred to obtain a mixed solution, and then the mixed solution is ultrasonically dispersed and then transferred to a storage tank for standby use.
[0020] Furthermore, the mass ratio of the ground glass fiber to the water-soluble resin glue is 1:10 to 4:1.
[0021] Furthermore, in step 4, the mixed solution of the ground glass fibers and the water-soluble resin glue is continuously stirred during storage in the storage tank to maintain the ground glass fibers in a suspended state in the water-soluble resin glue.
[0022] Preferably, in step 6, the ground glass fiber water-soluble resin glue is heated and cured in a hot air circulation curing furnace or cured in a microwave curing device. The hot air circulation curing furnace is divided into two stages:
[0023] The first stage: dehumidification stage, the temperature is 50℃~100℃, and it lasts for 30~150 minutes;
[0024] The second stage: curing stage, the temperature is 150-250℃, and it lasts for 50-200 minutes;
[0025] When using a microwave oven for curing, use a power of 250W to 1000W and microwave drying for 3 hours.
[0026] The ground glass fibers and the water-soluble resin adhesive provided by the present invention are uniformly dispersed in the product, and the non-woven layers are connected by needle-punching hooks and bonded by water-soluble resin adhesive to enhance the vertical tensile strength.
[0027] The beneficial effects of the present invention are as follows:
[0028] 1. The present invention evenly disperses the ground glass fibers in the glass fiber fireproof insulation board. The addition of the ground glass fibers can reduce the number and diameter of the holes inside the glass fiber fireproof insulation board, and can effectively hinder the convection heat transfer of the gas, thereby reducing the thermal conductivity of the glass fireproof insulation board. It has been verified that after adding the ground glass fibers, the thermal conductivity of the insulation board made of the same glass fiber mesh and water-soluble resin glue is reduced from 0.035w / (m*k) to 0.025w / (m*k), a reduction of about 30%.
[0029] 2. The present invention provides glass fibers in glass fiber mats of preferred sizes, ground glass fibers within a specific size range, and an optimal combination ratio of glass fibers in glass fiber mats. The thermal conductivity coefficient of the obtained product fluctuates less and the thermal insulation performance of the product is stable.
[0030] 3. The present invention increases the glass fiber content in the insulation board by grinding the glass fiber. More than 90% of the production raw materials are glass fibers, which are inorganic materials and do not have combustion performance. They have Class A fireproofing ability and can be widely used in the exterior walls of high-rise buildings.
[0031] 4. The present invention adopts a non-woven method in the production process. Each layer of fibers has a two-dimensional chaotic structure, and the layers are connected by needle hooks. Due to the existence of internal holes, it has good sound insulation and sound absorption properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a ground glass fiber modified glass fiber fireproof insulation board; wherein, the vertical downward line from the top indicates the pre-puncture path from top to bottom, and the vertical upward line from the bottom indicates the barbed path from bottom to top;
[0033] Among them: 1-fireproof insulation board, 2-milled glass fiber, 3-glass fiber mat, 4-single-layer fiber mesh. DETAILED DESCRIPTION
[0034] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. The present invention is described in detail below in conjunction with the embodiments and drawings. The protection scope of the present invention is not limited to the embodiments, and any changes made by those skilled in the art within the scope defined by the claims also fall within the protection scope of the present invention.
[0035] In this embodiment, the thermal conductivity is tested using the guarded hot plate method specified in GBT10294-2008, Determination of Steady-State Thermal Resistance and Related Properties of Thermal Insulation Materials.
[0036] The milled glass fiber is selected from one or more of alkali-free glass fiber, medium-alkali glass fiber, high-alkali glass fiber and alkali-resistant glass fiber, and is produced by a ball mill. During production, it is pre-mixed with a water-soluble resin and then evenly sprayed on the fiber web during web laying. In this embodiment, the milled fiber used is the alkali-free glass fiber (E) produced by Taishan Glass Fiber Co., Ltd., and the sizes are as follows:
[0037]
[0038] In this embodiment, the water-soluble resin comes from Aike-Tel Corporation, and its model number is EXP725272M.
[0039] The glass fibers used in this implementation case are hydrophobic glass fibers produced by Taishan Glass Fiber Co., Ltd., including but not limited to starch-based, water-drawn, thermoplastic chopped products, etc., which are:
[0040]
[0041]
[0042] Embodiment: A production line for grinding glass fiber modified high-strength continuous glass fiber fireproof insulation board
[0043] Step 1, loading:
[0044] After various glass fibers are weighed evenly according to the ratio, they are put into the automatic feeder, and the total control device sets the output, preferably controlling the output to 300Kg / h-400Kg / h. After the feeding amount is controlled by the feeding beater, they are sent to the rough opening through the belt. In the specific embodiment, the output is controlled to 350Kg / h.
[0045] Step 2: Fluffy treatment
[0046] (1) Rough opening
[0047] The glass fiber delivered by the bag opening equipment is opened in the opener and transported to the next process through the cotton conveying fan. Feed sheet metal with a thickness of 3mm; the input curtain is a PVC rubber curtain; the feeding roller is fed by double licker-in rollers, and the roller diameter is 80mm; the opening cylinder diameter is 400mmmm, and the needle clothing is wound on it, and the speed is 800-1000 rpm; the cotton conveying fan is controlled by a separate motor frequency conversion, and the air volume can be adjusted according to the output. The raw materials after rough opening are transported to the next large warehouse mixing equipment through the cotton conveying fan and pipeline. In the application, the sheet metal can be selected from 2mm-5mm thickness, roller diameter 70mm-90mm, and opening cylinder diameter 400mm-500mm.
[0048] The large-bin cotton mixing equipment fully mixes and stores the coarsely opened glass fibers in the large-bin cotton mixing equipment to achieve continuous production. The large-bin cotton mixing equipment is a common equipment in this field, including a cotton box, a conveying curtain, a diagonal nail curtain, a beater, a condenser, and a photoelectric control system.
[0049] Two sets of condensers are installed above the cotton box for mixing cotton in the large warehouse. Dust suction interfaces are installed on the condensers and punching parts and connected to the central dust removal unit.
[0050] (2) Fine opening
[0051] Fine opening equipment further opens the glass fiber sent from the large warehouse in the opening and conveying machine, and transports it to the next process through the cotton conveying fan. The raw materials of the fine opening equipment are transported to the vibrating cotton box through the cotton conveying fan and pipeline, and then transported to the carding machine through the belt scale.
[0052] Step 3: Organize the network
[0053] The carding equipment mixes the opened glass fibers evenly on the carding machine, and then outputs them after being mixed by the feeding roller, the chest cylinder, the transfer roller, and the inner and outer shuffles to obtain a fiber web. The weight of the obtained fiber web single layer is 80-140g / m 2 .
[0054] Step 4: Glue and mesh laying.
[0055] (1) Preparation of adhesive solution
[0056] The weighed ground glass fiber is uniformly added into the water-soluble resin at room temperature, the mass ratio of the ground glass fiber to the water-soluble resin glue is 1:10-4:1, the solid content of the water-soluble resin glue is 35%-55%, and an agitator is used to stir at a speed of 15rpm-30rpm for 5 minutes. The mixed liquid is transferred to an ultrasonic vibration device, dispersed at a frequency of 35KHZ-40KHZ for 5 minutes, and then transferred to a storage tank for standby use. At the same time, there is a stirring device in the storage tank, and it is stirred at 5rpm-10rpm during storage to obtain a glue solution.
[0057] (2) Glue spraying
[0058] The spraying equipment is designed with a uniform glue application (spraying) device, which is installed on the web laying trolley of the web laying machine to spray glue on the fiber web continuously and evenly with the reciprocating motion of the web laying trolley. The glue liquid is placed in a storage tank, and the glue liquid is transported to the diversion control device through a multi-stage centrifugal pump, and then the glue liquid is diverted to the delivery pipes of each nozzle. The nozzle delivery pipe is arranged according to the number of nozzles to spray glue on the fiber web; the accuracy and uniformity of glue application (spraying) in the continuous production process are precisely controlled by adjusting the pressure and flow of the multi-stage centrifugal pump, setting the parameters of the diversion control device, and selecting the nozzle specifications. The spraying flow is 14Kg / h, and the web laying speed during production is 38m / min. Through the reciprocating motion of the web laying trolley, the fiber web sprayed with glue is continuously laid in multiple layers on the bottom curtain to form a glue-sprayed fiber web layer, which is then transported to the next process.
[0059] Step 5: Needle punching
[0060] Pre-puncture: The fiber web layer obtained in step 4 is compressed and punctured from top to bottom with a needle at a puncture frequency of 150 rpm and a puncture depth of 45.1 mm to preliminarily strengthen the strength of the fiber web layer.
[0061] Barbed: The pre-punctured fiber web layer is needled from bottom to top with needles, the needle frequency is 150rpm, the needle depth is 5.4mm, to further strengthen the strength of the web layer, to form a glue-containing needle-punched felt embryo, and the glass fibers around the ground glass fibers exist in the form of needle-punched hooked glass fibers. The felt output from the pre-punctured machine enters the barb-punched machine through the input curtain of the barb-punched machine.
[0062] Step 6, Curing
[0063] Use hot air circulation curing furnace to curing and shaping the rubber blank. According to the product specifications and production capacity requirements, calculate the effective length of the hot air circulation curing furnace equipment, production line speed, number and power of the hot air circulation system, power and flow of each fan and other parameters, so as to determine the technical requirements of the drying and curing equipment.
[0064] Furthermore, it was determined that the production line speed adjustment range of the equipment is 0.2m-5m / min, the product width adaptation range is 1000mm-2000mm, and the product thickness adaptation range is 10mm-100mm. The hot air circulation curing furnace is divided into two stages:
[0065] The first stage: dehumidification stage, the temperature is 50°C to 100°C, and it lasts for 30 to 150 minutes. In the embodiment described below, the temperature is controlled at 80°C and it lasts for 90 minutes.
[0066] The second stage: curing stage, hot air circulation curing temperature is 150-250°C, lasting for 50-200 minutes. In the embodiment described below, the temperature is controlled to be 200°C, lasting for 100 minutes.
[0067] If using a microwave oven for curing, use a power of 250W to 1000w and microwave drying for 3 hours.
[0068] Step 7, sizing
[0069] The dried and solidified products are cut horizontally and vertically to produce fireproof insulation boards of specific sizes.
[0070] Comparative Example 1: Fiberglass Fireproof Insulation Board
[0071] Preparation method: Remove the step 4 of adding ground glass fiber in the embodiment and directly use water-soluble resin to produce ordinary glass fiber fireproof insulation board.
[0072] Comparative Example 2: Rockwool Insulation Board
[0073] Preparation method: Purchase rock wool insulation boards from other manufacturers.
[0074] Test Example 1: Insulation Boards Made of Different Grinded Glass
[0075] The fireproof insulation board was prepared according to the steps of the embodiment using milled glass fibers of different size parameters. The performance test results of the fireproof insulation board products obtained in Comparative Example 1 and Comparative Example 2 are shown in the following table:
[0076] Table 1 Comparison of the performance of insulation boards made of different ground glasses
[0077]
[0078]
[0079] The results show that, under the premise that the raw materials of glass fiber mesh and water-soluble resin glue are the same, the thermal conductivity coefficients of fireproof insulation boards made of milled glass fibers with different size parameters are different, among which the thermal conductivity coefficient of the insulation board obtained by "milled glass fiber 2" (length 50μm, diameter 9μm) is lower than that of smaller or larger milled glass fibers. In addition, the thermal conductivity coefficient of milled glass fiber 4 with a length of 150μm and a diameter of 80μm is not superior to that of rock wool fiber. It is considered that its length is too large, and it is easy to produce gaps due to hooking during the needling process, which makes the total volume of the gaps larger, which contributes to a certain improvement in the thermal conductivity effect, resulting in an increase in the thermal conductivity coefficient.
[0080] Test Example 2: Insulation Boards Made from Different Glass Fiber Raw Materials
[0081] Glass fibers with different size parameters were used as fiber meshes to prepare fireproof insulation boards according to the steps of the embodiment. The test results of various properties of the obtained fireproof insulation board products are shown in the following table:
[0082] Table 2 Performance indicators of insulation boards made from different glass fiber raw materials
[0083]
[0084]
[0085] According to the results, compared with other ratios, the thermal conductivity of the fireproof insulation board made of raw material-2 is lower. The possible reasons are: the overall fiber diameter of raw material-2 is lower, and after the fibers are combed into a web, the pores of the fiber web are smaller, which can significantly weaken the gas convection heat transfer in the heat transfer process.
[0086] Test Example 3: Insulation Boards Made of Ground Glass in Different Ratios
[0087]
[0088] The results show that
[0089] 1. When adding the same amount of milled glass fiber, the milled glass fiber modified glass fiber fireproof insulation board produced by raw material-2 has the lowest thermal conductivity and the best performance.
[0090] 2. When using the same raw fiber ratio, the addition of ground glass fiber-2 can effectively reduce the glass fiber fireproof insulation board.
[0091] 3. When the content of ground glass fiber is low (<1%), it has almost no effect on the thermal conductivity of the glass fiber fireproof insulation board; when the content of ground glass fiber is high (>15%), the results show that the thermal conductivity of the glass fiber fireproof insulation board increases. The reason may be that when there are too many ground glass fibers, the holes are blocked, and the insulation board is directly heat-conducted, and the thermal conductivity effect is improved. Therefore, the optimal addition amount of ground glass fiber is 1% to 15%, and more preferably 1% to 5%. The thermal conductivity of the product within this range fluctuates less, and the thermal insulation performance is more stable.
[0092] In addition, when the length and diameter of the added ground glass fiber are too large, it is easy to cause the internal pores of the glass fiber to be blocked in the glass fiber fireproof insulation board, increase heat conduction, and then lead to an increase in thermal conductivity, affecting the overall performance of the product.
[0093] The products obtained by the present invention are as follows Figure 1 As shown, the fireproof insulation board 1 includes a glass fiber mat 3 formed by plying multiple layers of single-layer fiber mesh 4, a water-soluble resin is impregnated in the glass fiber mat 3, and ground glass fibers 2 are dispersed in the glass fiber mat and the water-soluble resin glue.
[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A fireproof insulation board with ground glass added, characterized in that: The invention comprises the following components: ground glass fibers in the form of ground glass, glass fibers in the form of glass fiber mats, and water-soluble resin glue, wherein the ground glass fibers are dispersed in the glass fiber mats and the water-soluble resin glue; Wherein, the glass fiber content in the glass fiber mat is 80% to 97%, and the content of the water-soluble resin glue is 2.5% to 15%; The milled glass fibers are selected from 30 to 50 μm in length and 3 to 9 μm in diameter; The glass fiber in the glass fiber mat is a combination of two types of glass fibers, one type of which has a length of 50 mm to 100 mm and a diameter of 8 μm to 10 μm, and the other type of which has a length of 50 mm to 100 mm and a diameter of 5 μm to 7 μm; The content of the ground glass fiber is 1% to 5%.
2. The fireproof insulation board with ground glass added according to claim 1, characterized in that: The ground glass fiber component is selected from one or more of alkali-free glass fiber, medium-alkali glass fiber, high-alkali glass fiber and alkali-resistant glass fiber; the glass fiber component in the glass fiber mat is alkali-free glass fiber.
3. The fireproof insulation board with ground glass added according to claim 1, characterized in that: The milled glass fiber is made of E glass milled fiber, has a length of 50 μm and a diameter of 8 μm.
4. The fireproof insulation board with ground glass added according to claim 1, characterized in that: The thickness of the fireproof heat-insulating board product with added ground glass is between 4 mm and 150 mm.
5. A method for preparing a fireproof insulation board with ground glass, characterized in that: The fireproof insulation board with ground glass added comprises the following components: ground glass fiber in the form of ground glass, glass fiber in the form of glass fiber mat and water-soluble resin glue, wherein the ground glass fiber is dispersed in the glass fiber mat and the water-soluble resin glue; wherein the glass fiber content in the glass fiber mat is 80% to 97%, and the content of the water-soluble resin glue is 2.5% to 15%; the ground glass fiber is selected from a length of 30 to 50 μm and a diameter of 3 to 9 μm; the glass fiber in the glass fiber mat is a combination of two types of glass fibers, wherein one type is 50 mm to 100 mm in length and 8 μm to 10 μm in diameter, and the other type is 50 mm to 100 mm in length and 5 μm to 7 μm in diameter; the content of the ground glass fiber is 1% to 5%; The steps include: Step 1, loading; Step 2, fluffing treatment, rough opening and fine opening treatment are performed in the opening machine; Step 3: finishing the net, and processing it in a finishing machine to obtain a fiber net, the single-layer net weight of the fiber net is 80-140g / m 2 ; Step 4, applying glue and laying the web, spraying the water-soluble resin glue added with the ground glass fiber onto the fiber web obtained in step 3, and laying the glue-sprayed fiber web in multiple layers continuously to form a glue-sprayed fiber web layer; Step 5, needle-punching into felt, needle-punching the spray-bonded fiber mesh layer obtained in step 4, including pre-puncturing from top to bottom and barbing from bottom to top, to obtain a glass fiber felt; Step 6, curing, curing the glass fiber mat obtained in step 5 into shape.
6. The method for preparing a fireproof heat-insulating board with ground glass added according to claim 5, characterized in that: In step 4, the ground glass fiber is first added to the water-soluble resin glue and stirred to obtain a mixed solution, and then the mixed solution is ultrasonically dispersed and then transferred to a storage tank for standby use; the mixed solution of the ground glass fiber and the water-soluble resin glue is stirred continuously during storage in the storage tank to maintain the ground glass fiber in a suspended state in the water-soluble resin glue.
7. The method for preparing a fireproof heat-insulating board with ground glass added according to claim 6, characterized in that: The mass ratio of the ground glass fiber to the water-soluble resin glue is 1:10 to 4:1.
Citation Information
Patent Citations
Novel thermal insulation board and preparation process thereof
CN112142367A
Milled fiber and glass fiber net cover containing same, and manufacture method thereof
CN102775639A
Milled glass fiber production process
CN103894275A
Wear-resistant corrosion-resistant grade level and preparation method thereof
CN109367168A
Laminated glass fiber felt material
CN110183753A