Aluminum-magnesium dry ramming material for medium frequency induction furnace and preparation method thereof
By introducing spinel-calcium aluminate composite materials into the alumina-magnesium dry ramming materials, the spinel chemical reaction and strengthening material combination are controlled, and the resistance of the alumina-magnesium dry ramming materials in the medium frequency induction furnace is solved. The problem of insufficient slag performance has been significantly improved, its strength and resistance to slag penetration have been significantly improved, and the service life of the furnace lining has been extended.
Patent Information
- Application Number
- CN202310060815.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-19
AI Technical Summary
The existing aluminum-magnesium dry ramming materials are prone to spinelization in medium frequency induction furnaces, leading to expansion, structural damage, and insufficient slag resistance, which affects the service life and strength of the furnace lining.
The spinel-calcium aluminate composite phase material is introduced to regulate the in-situ spinelization reaction, strengthen the material combination, form an excellent three-phase structure, and improve the slag resistance performance.
It significantly reduces the line change after burning, improves the strength and slag penetration resistance of the aluminum-magnesia dry ramming material, and extends the service life of the furnace lining.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of refractory materials for medium frequency induction furnace bodies, and in particular to an aluminum-magnesium dry ramming material for a medium frequency induction furnace and a preparation method thereof. Background Art
[0002] Medium frequency induction furnaces are widely used in the foundry industry and in the smelting of alloy steel, carbon steel and various high-performance steel grades due to their flexibility, environmental protection and high efficiency. The lining is one of the most important components of the induction furnace, which plays the role of holding molten metal and protecting the furnace body. With the requirements of high-quality steelmaking technology, the requirements for lining materials are becoming more and more stringent. During the smelting process, the lining itself is in an extremely harsh environment, facing a series of problems that seriously shorten the service life of the lining, such as the impact of molten metal, the penetration of metal ions, and the thermal stress caused by rapid temperature changes. The quality of the lining directly determines its production efficiency and service life. With the rapid development of short-process steelmaking, the demand for high-quality dry ramming materials for medium frequency induction furnaces is also increasing. Especially when smelting low-alloy steel in an induction furnace, the MnO content in the slag is high, and the penetration of the lining material is serious, which has become a technical problem that needs to be solved urgently.
[0003] At present, aluminum-magnesium dry ramming mass is a commonly used dry ramming mass, which usually uses corundum and magnesia as raw materials. This traditional aluminum-magnesium dry ramming mass faces abnormal expansion caused by in-situ spinelization during use, which destroys the structure of the material and makes it easier for the aluminum-magnesium dry ramming mass to be penetrated by slag during use, thereby reducing the service life of the furnace lining. And this traditional aluminum-magnesium dry ramming mass has the disadvantages of high porosity, loose structure, and low strength. Therefore, how to improve the physical properties and anti-permeability properties of aluminum-magnesium dry ramming mass is the focus of developing high-performance aluminum-magnesium dry ramming mass.
[0004] The Chinese patent document with application number 201811645498.1 reports an aluminum-magnesium dry ramming material and a preparation method thereof, wherein the components of the ramming material include fused corundum particles and fine powder, magnesia particles and fine powder, plate-shaped corundum particles, boric acid, and a high-temperature composite sintering promoter composed of silicon powder and SiC. The invention improves the thermal shock resistance and chemical corrosion resistance of the ramming material through reasonable particle grading, and cooperates with the sintering process to form spinel in the furnace lining during use, and the resulting expansion matches the contraction caused by sintering, thereby improving the sintering quality of the medium frequency furnace lining after construction and making the overall strength of the furnace lining better. However, the introduction of silicon element in the invention is not conducive to the high temperature strength and slag resistance of the aluminum-magnesium dry ramming material.
[0005] The Chinese patent document with application number 201610667100.9 reports a ramming material for a medium frequency induction furnace and a preparation method thereof, wherein the components of the ramming material include fused white corundum, fused magnesia, alumina powder, aluminum lactate and magnesium lactate, and the aluminum oxide and magnesium oxide obtained by decomposing aluminum lactate and magnesium lactate are sintered at a lower temperature, thereby optimizing the high temperature performance of the ramming material. However, the obtained ramming material has low volume density and strength, and large linear variation.
[0006] The Chinese patent application number 202210437255.9 discloses a high-strength chrome corundum ramming mass, which includes the following raw materials by mass percentage: 25-35% magnesium aluminum spinel particles, 3-5% silicon nitride, 4-6% active α-Al2O3 powder, 5-8% magnesium oxide, 4-6% binder, 1-3% inhibitor, 0.1-0.3% explosion-proof fiber, and the balance is chrome corundum. The ramming mass has the characteristics of high strength, good wear resistance, good resistance to coal slag erosion and good resistance to coal slag penetration, but the preparation process of its binder and inhibitor is complicated, and the ramming mass contains chromium that is harmful to the human body and the environment.
[0007] The aluminum-magnesium dry ramming material of the present invention introduces a spinel-calcium aluminate composite material, uses pre-synthesized spinel to regulate the in-situ spinelization reaction in the aluminum-magnesium dry ramming material, and uses calcium aluminate to strengthen the combination of the matrix and the aggregate, so that the physical properties of the ramming material are greatly improved, especially the reduction of the line change after burning and the improvement of the anti-slag penetration performance. The method is expected to become one of the important ways to develop high-performance aluminum-magnesium dry ramming materials. Summary of the invention
[0008] The present invention aims to overcome the above-mentioned technical problems of aluminum-magnesium dry ramming mass in the prior art, and aims to provide an aluminum-magnesium dry ramming mass for a medium frequency induction furnace and a preparation method thereof. By introducing a spinel-calcium aluminate composite material, the in-situ spinelization reaction and the strengthening of the bonding in the aluminum-magnesium dry ramming mass are regulated, and vacancy defects are formed to absorb MnO in the slag, thereby improving the slag permeability resistance and obtaining a ramming mass with excellent physical properties and high permeability resistance.
[0009] In order to solve the technical problems in practical applications, the technical solution adopted by the present invention is:
[0010] The present invention provides an aluminum-magnesium dry ramming mass for a medium frequency induction furnace, wherein the aluminum-magnesium dry ramming mass contains a spinel-calcium aluminate composite material. Specifically, every 100 parts by mass of the aluminum-magnesium dry ramming mass consists of 70-80 parts by mass of fused white corundum, 10-15 parts by mass of magnesia, 1-5 parts by mass of plate-shaped corundum, 1-5 parts by mass of calcined alumina, and 1-15 parts by mass of the spinel-calcium aluminate composite material.
[0011] Preferably, in addition to the above-mentioned components, the aluminum-magnesium dry ramming material also contains 0.5-2 parts by mass of a binder.
[0012] The aluminum-magnesium dry ramming mass is prepared by uniformly mixing the above raw materials to obtain the aluminum-magnesium dry ramming mass for a medium frequency induction furnace.
[0013] Furthermore, the purity of the fused white corundum is ≥98%, and its particle gradation is: 3-5mm fused white corundum is 10-20 mass parts of the ramming material, 1-3mm fused white corundum is 30-40 mass parts of the ramming material, 0-1mm fused white corundum is 20-30 mass parts of the ramming material, and <74μm fused white corundum is 5-10 mass parts of the ramming material.
[0014] The magnesia is sintered magnesia with a purity of ≥97%. The sintered magnesia with a particle size of <74 μm accounts for 1-10 parts by mass of the ramming material, and the sintered magnesia with a particle size of <0.3 mm accounts for 5-15 parts by mass of the ramming material.
[0015] The purity of the plate-shaped corundum is ≥99% and the particle size is <45 μm.
[0016] The purity of the calcined alumina powder is ≥99%; the particle size d 50 4-6μm.
[0017] The preferred spinel-calcium aluminate composite material has an Al2O3 content of 69-71wt%, a MgO content of 16-22wt%, and a CaO content of 8-11wt%; it is composed of 60-72wt% spinel, 18-22wt% calcium monoaluminate and 8-12wt% calcium dialuminate; its particle size distribution <1mm particles account for 1-15 mass parts of the ramming material, and further, particles <74μm account for 1-15 mass parts of the ramming material.
[0018] The binder has a specific gravity of> 1.15 g / cm 3 dextrin solution or 10% polyvinyl alcohol (PVA) solution.
[0019] The mixing is performed by premixing fine powder raw materials including plate-shaped corundum, calcined alumina, sintered magnesia and spinel-calcium aluminate composite material in a mixer for 15-30 minutes, and then adding fused white corundum aggregate, or fused white corundum aggregate and binder (when binder is included in the components) and mixing for 15-30 minutes.
[0020] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0021] The main phases of the spinel-calcium aluminate composite material used in the present invention are magnesium aluminum spinel and calcium aluminate. Magnesium aluminum spinel has good slag resistance and high temperature performance and is a good refractory material. On the one hand, the addition of pre-synthesized spinel can reduce the expansion caused by the in-situ spinelization reaction, reduce the cracking and peeling of the furnace lining, increase the service life of the furnace lining, and reduce the consumption of the furnace lining material. In addition, the calcium aluminate material, corundum and spinel form an excellent bonding system at high temperature, which strengthens the bonding within the matrix and between the matrix and the aggregate. In particular, calcium hexaaluminate is generated by the reaction at the edge of the corundum aggregate, which can tightly connect the spinel in the matrix with the corundum aggregate to strengthen the bonding between the aggregate and the matrix, forming a tightly bonded corundum / calcium hexaaluminate / spinel structure. The mechanical properties of this three-phase structure are better than those of the corundum-spinel structure. At the same time, due to the introduction of the spinel-calcium aluminate composite material, the Al2O3 / MgO ratio in the matrix changes. The spinel formed in situ from the magnesia reaction and the pre-synthesized spinel in the composite material both dissolve more alumina as the reaction progresses and the temperature rises; the aluminum-rich spinel formed thereby contains more vacancy defects and can absorb more MnO and Fe2O3 in the slag, thereby enhancing the slag resistance of the material. Therefore, by introducing the spinel-calcium aluminate composite material into the aluminum-magnesium dry ramming material, the post-sintering linear change of the aluminum-magnesium dry ramming material containing the spinel-calcium aluminate composite material can be significantly reduced, and its strength and slag penetration resistance can be improved. The aluminum-magnesium dry ramming material provided by the present invention has significantly better resistance to the permeability of manganese-containing slag than the traditional aluminum-magnesium dry ramming material without the addition of spinel-calcium aluminate complex phase material. The aluminum-magnesium dry ramming material containing the spinel-calcium aluminate complex phase material provided by the present invention is tested: the line change after burning is 2.11%, the compressive strength is 11.5MPa, and the permeability index is 22.98%; the aluminum-magnesium dry ramming material without the addition of spinel-calcium aluminate complex phase material is tested: the line change after burning is 3.48%, the compressive strength is 9.0MPa, and the permeability index is 34.94%.
[0022] Therefore, the aluminum-magnesium dry ramming material containing spinel-calcium aluminate composite material prepared by the present invention can be produced on a large scale industrially, and has excellent strength, slag permeability resistance and low linear variation, and is suitable for medium frequency induction furnace lining; in particular, it is suitable for induction furnace smelting of low-alloy steel with high manganese content in slag. DETAILED DESCRIPTION
[0023] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0024] The present invention will be further described below in conjunction with the embodiments.
[0025] The common points in the raw materials involved in each embodiment are described as follows, which will not be repeated in the embodiments. The purity of the fused white corundum used in each embodiment is ≥98%, that is, the Al2O3 content is ≥98%; the magnesia is sintered magnesia, and its purity is ≥97%; the purity of the plate-shaped corundum is ≥99%, that is, the Al2O3 content is ≥98%, and the particle size is <45μm; the Al2O3 content of the calcined alumina powder is ≥99%; the Al2O3 content of the spinel-calcium aluminate composite material in Examples 1-3 is 70wt%; the MgO content is 20.5wt%; and the CaO content is 8.5wt%. The mass parts of each raw material added in the following embodiments refer to the mass parts per 100 parts of ramming material.
[0026] Example 1
[0027] The aluminum-magnesium dry ramming material of this embodiment is prepared using the following raw materials.
[0028] The fused white corundum is 79 parts by mass, of which the content of particle size <74 μm, 1-3 mm, and 3-5 mm is 7 parts by mass, 35 parts by mass, and 14 parts by mass respectively, and the content of 0-1 mm is 23 parts by mass.
[0029] The sintered magnesia is 11 parts by mass, of which 4 parts by mass are sintered magnesia with a particle size of <0.074 mm, and 7 parts by mass are sintered magnesia with a particle size of <0.3 mm.
[0030] 3 parts by mass of tabular corundum.
[0031] Calcined alumina particle size d 50 =5 μm, 3 parts by mass.
[0032] The fine powder of the spinel-calcium aluminate composite material with a particle size of less than 74 μm is 4 parts by mass.
[0033] A 10% polyvinyl alcohol (PVA) solution is used as a binder, and the mass ratio of the added amount to the total amount of the above raw materials is 2:100.
[0034] Example 2
[0035] The aluminum-magnesium dry ramming material of this embodiment is prepared using the following raw materials.
[0036] The fused white corundum is 75 parts by mass, of which the content of particle size <74μm, 1-3mm, and 3-5mm is 7 parts by mass, 35 parts by mass, and 14 parts by mass respectively, and the content of 0-1mm is 19 parts by mass.
[0037] The sintered magnesia is 7 parts by mass, of which: 4 parts by mass of sintered magnesia with a particle size of <0.074 mm, and 3 parts by mass of sintered magnesia with a particle size of <0.3 mm.
[0038] 3 parts by mass of tabular corundum.
[0039] Calcined alumina particle size d 50 =5 μm, 3 parts by mass.
[0040] The spinel-calcium aluminate composite material fine powder with a particle size of less than 74 μm is 4 parts by mass, and the other spinel-calcium aluminate composite material particles smaller than 1 mm are 8 parts by mass.
[0041] A 10% polyvinyl alcohol (PVA) solution is used as a binder, and the mass ratio of the added amount to the total amount of the above raw materials is 2:100.
[0042] Example 3
[0043] The aluminum-magnesium dry ramming material of this embodiment is prepared using the following raw materials. No binder is added in this embodiment.
[0044] The fused white corundum is 79 parts by mass, of which the content of particle size <74 μm, 1-3 mm, and 3-5 mm is 7 parts by mass, 35 parts by mass, and 14 parts by mass respectively, and the content of 0-1 mm is 23 parts by mass.
[0045] The sintered magnesia is 11 parts by mass, of which 4 parts by mass are sintered magnesia with a particle size of <0.074 mm, and 7 parts by mass are sintered magnesia with a particle size of <0.3 mm.
[0046] 3 parts by mass of tabular corundum.
[0047] Calcined alumina particle size d 50 =5 μm, 3 parts by mass.
[0048] The fine powder of the spinel-calcium aluminate composite material with a particle size of less than 74 μm is 4 parts by mass.
[0049] Other embodiments
[0050] On the basis of the above embodiments, the inventor adjusted the raw material parameters to prepare a series of aluminum-magnesium dry ramming materials, and the raw material parameters were adjusted within the following ranges:
[0051] In the prepared series of aluminum-magnesium dry ramming materials, every 100 parts by mass of the aluminum-magnesium dry ramming materials are composed of 70-80 parts by mass of fused white corundum, 10-15 parts by mass of magnesia, 1-5 parts by mass of plate-like corundum, 1-5 parts by mass of calcined alumina, and 1-15 parts by mass of spinel-calcium aluminate composite material.
[0052] The particle size distribution of fused white corundum is as follows: 10-20 parts by mass of 3-5mm fused white corundum, 30-40 parts by mass of 1-3mm fused white corundum, 20-30 parts by mass of 0-1mm fused white corundum, and 5-10 parts by mass of <74μm fused white corundum.
[0053] The proportion of sintered magnesia is: 1-10 parts by mass of sintered magnesia with a particle size of less than 74 μm, and 5-15 parts by mass of sintered magnesia with a particle size of less than 0.3 mm in the ramming material.
[0054] The particle size of the calcined alumina powder is 50 4-6μm.
[0055] The spinel-calcium aluminate composite material has an Al2O3 content of 69-71wt%, a MgO content of 16-22wt%, and a CaO content of 8-11wt%; it is composed of 60-72wt% spinel, 18-22wt% calcium monoaluminate, and 8-12wt% calcium dialuminate; its particle size distribution has 0-1mm particles of 1-15 parts by mass, including 1-15 parts by mass of particles <74μm.
[0056] The inventor adjusted the raw materials within the above range to prepare a series of aluminum-magnesium dry ramming materials. In the final slag resistance test, strength and other physical properties, the test results were comparable to the performance data of the aluminum-magnesium dry ramming materials obtained in Examples 1-3. Adjustment within the above range can achieve the purpose of the present invention.
[0057] In addition, on the basis of the above raw materials, the inventors also added 0.5-2 parts by mass of a binder based on the total mass of the above raw materials, and also prepared a series of aluminum-magnesium dry ramming materials. The performance test results showed that the addition of the binder had no significant effect on the performance, and the purpose of the present invention could be achieved after adding the binder.
[0058] The inventors used the following process to prepare the aluminum-magnesium dry ramming materials of the above embodiments:
[0059] Step 1): Premix fine powder raw materials including plate-like corundum, calcined alumina, sintered magnesia and spinel-calcium aluminate composite material in a mixer for 15-30 minutes, and then add fused white corundum aggregate, or fused white corundum aggregate and binder (in the embodiment where the components contain a binder) and mix for 15-30 minutes.
[0060] Step 2): Ramming or pressing the mixed material into a shape, drying it at 110° C. for 24 hours, and then keeping it at 1600° C. for 3 hours, to obtain the aluminum-magnesium dry ramming material of the present invention.
[0061] Comparative Example
[0062] Ordinary aluminum-magnesium dry ramming material and preparation method thereof. The ordinary aluminum-magnesium dry ramming material of this comparative example adopts raw material composition: 7 weight parts, 35 weight parts and 14 weight parts of fused white corundum with particle size of <74m, 1-3mm and 3-5mm respectively, 23 weight parts of 0-1mm fused white corundum; 8 weight parts of sintered magnesia with particle size of <0.074mm, 7 weight parts of sintered magnesia with particle size of <0.3mm; 3 weight parts of plate-shaped corundum; calcined alumina particle size d 50 =5μm, 3 parts by mass. After premixing plate-shaped corundum, calcined alumina and sintered magnesia for 15-30 minutes, add fused white corundum aggregate and mix for 15-30 minutes; ram or press the mixed materials, first dry at 110°C for 24 hours, and then keep at 1600°C for 3 hours to obtain the aluminum-magnesium dry ramming material of this comparative example.
[0063] Performance Test:
[0064] The aluminum-magnesium dry ramming materials prepared in the above embodiments and comparative examples were subjected to various performance tests, wherein the static crucible method was used to conduct the slag resistance test, and the erosion of the ramming materials by the slag was evaluated after being kept at 1600°C for 3 hours. The chemical composition of the slag is shown in Table 1, from which it can be seen that the MnO content in the slag is relatively high, which is the main reason for the serious penetration of the slag into the furnace lining material, especially when smelting low alloy steel in an induction furnace.
[0065] Table 1 Chemical composition of slag (wt%)
[0066] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[Na2O]]> <![CDATA[TiO2]]> MnO 58.75 7.95 3.25 0.64 0.12 1.31 0.75 27.22
[0067] The test results of the aluminum-magnesium dry ramming material prepared in Example 1 are as follows: the line change after burning is 2.50%, the compressive strength is 9.9 MPa, and the permeability index is 30.26%.
[0068] The test results of the aluminum-magnesium dry ramming material prepared in Example 2 are as follows: the linear change after firing is 2.11%, the compressive strength is 11.52 MPa, and the permeability index is 22.98%.
[0069] The test results of the aluminum-magnesium dry ramming materials prepared in other embodiments have comparable performance to those of embodiments 1 and 2, and are not listed in detail here.
[0070] In comparison, the test results of the aluminum-magnesium dry ramming material prepared in the comparative example without the spinel-calcium aluminate composite material are as follows: the linear change after firing is 3.48%, the compressive strength is 9.0 MPa, and the permeability index is 34.94%.
[0071] Table 2 Performance of aluminum-magnesium dry ramming materials of Examples 1-2 and Comparative Examples
[0072] 1600℃×3h Comparative Example Example 1 Example 2 Line change after burning (%) 3.48 2.5 2.11 Room temperature compressive strength (MPa) 9.0 9.9 11.52 Slag penetration index (%) 34.94 30.26 22.98
[0073] From the above data, it can be seen that the present invention introduces spinel-calcium aluminate composite material into aluminum-magnesium dry ramming material. Due to the introduction of spinel-calcium aluminate composite material, the Al2O3 / MgO ratio in the matrix changes, and the spinel formed in situ by the magnesia reaction and the pre-synthesized spinel in the composite material both dissolve more aluminum oxide as the reaction progresses and the temperature rises. The aluminum-rich spinel thus formed contains more vacancy defects, and can absorb more MnO and Fe2O3 in the slag, thereby enhancing the slag penetration resistance of the manganese-containing slag of the material. Therefore, by introducing spinel-calcium aluminate composite material into aluminum-magnesium dry ramming material, the post-burning line change of the aluminum-magnesium dry ramming material containing spinel-calcium aluminate composite material can be significantly reduced, and its strength and slag penetration resistance can be improved.
[0074] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. An aluminum-magnesium dry ramming material for a medium frequency induction furnace, characterized in that: Every 100 parts by mass of the aluminum-magnesium dry ramming material consists of 70-80 parts by mass of fused white corundum, 10-15 parts by mass of magnesia, 1-5 parts by mass of plate-like corundum, 1-5 parts by mass of calcined alumina, and 1-15 parts by mass of spinel-calcium aluminate composite material; or Every 100 parts by mass of the aluminum-magnesium dry ramming material consists of 70-80 parts by mass of fused white corundum, 10-15 parts by mass of magnesia, 1-5 parts by mass of plate-shaped corundum, 1-5 parts by mass of calcined alumina, 1-15 parts by mass of spinel-calcium aluminate composite material, and 0.5-2 parts by mass of a binder; The spinel-calcium aluminate composite material has an Al2O3 content of 69-71wt%, a MgO content of 16-22wt%, and a CaO content of 8-11wt%; and is composed of 60-72wt% spinel, 18-22wt% calcium monoaluminate, and 8-12wt% calcium dialuminate.
2. The aluminum-magnesium dry ramming material for a medium frequency induction furnace according to claim 1, characterized in that: The purity of the fused white corundum is ≥98%, and its particle gradation is: 10-20 mass parts of 3-5 mm fused white corundum in every 100 mass parts of the ramming material, 30-40 mass parts of 1-3 mm fused white corundum, 20-30 mass parts of 0-1 mm fused white corundum, and 5-10 mass parts of <74 µm fused white corundum.
3. The aluminum-magnesium dry ramming material for a medium frequency induction furnace according to claim 1, characterized in that: The magnesia is sintered magnesia with a purity of ≥97%. The sintered magnesia with a particle size of <74µm accounts for 1-10 parts by mass of every 100 parts by mass of the ramming material, and the sintered magnesia with a particle size of <0.3mm accounts for 5-15 parts by mass.
4. The aluminum-magnesium dry ramming material for a medium frequency induction furnace according to claim 1, characterized in that: The purity of the tabular corundum is ≥99% and the particle size is <45µm.
5. The aluminum-magnesium dry ramming material for a medium frequency induction furnace according to claim 1, characterized in that: The purity of the calcined alumina powder is ≥99%; the particle size d 50 4-6µm.
6. The aluminum-magnesium dry ramming material for a medium frequency induction furnace according to claim 1, characterized in that: The spinel-calcium aluminate composite material has a particle size distribution of <1 mm, and the particles have a particle size distribution of 1-15 parts by mass per 100 parts by mass of the ramming material, or particles of <74 µm, and the particles have a particle size distribution of 1-15 parts by mass per 100 parts by mass of the ramming material.
7. The aluminum-magnesium dry ramming material for a medium frequency induction furnace according to claim 1, characterized in that: The binder has a specific gravity of> 1.15 g / cm 3 dextrin solution or 10% polyvinyl alcohol solution.
8. A method for preparing an aluminum-magnesium dry ramming material for a medium frequency induction furnace according to any one of claims 1 to 7, characterized in that: In a mixer, plate-shaped corundum, calcined alumina, sintered magnesia and spinel-calcium aluminate composite material are premixed, and then fused white corundum aggregate or fused white corundum aggregate and binder are added to obtain the aluminum-magnesium dry ramming material.
9. Use of an aluminum-magnesium dry ramming mass for a medium frequency induction furnace according to any one of claims 1 to 7, wherein the aluminum-magnesium dry ramming mass is used for a lining of a medium frequency induction furnace.
10. Use of an aluminum-magnesium dry ramming mass for a medium frequency induction furnace according to claim 9, wherein the aluminum-magnesium dry ramming mass is used for a lining of a medium frequency induction furnace for smelting low alloy steel.
Citation Information
Patent Citations
High-strength chrome corundum ramming material and preparation method thereof
CN114538903A
Dry ramming material for bottom working lining of large ladle
CN106145964A
Ramming mass for medium-frequency induction furnace and preparing method thereof
CN106278315A
Corundum dry type ramming material for medium-frequency induction furnace and preparation method of corundum dry type ramming material
CN109320217A
Magnesia-carbon material containing spinel-calcium aluminate multiphase material and preparation method thereof
CN109369155A
Cited By
High-performance corundum dry ramming material for medium-frequency induction furnace and preparation method of high-performance corundum dry ramming material
CN117534493A
High-performance corundum dry ramming mix for medium-frequency induction furnace and preparation method thereof
CN117534493B