Method for extracting precious metals from precious metal-containing materials
By smelting and electrolyzing the precious metal-containing material with copper in an arc furnace, combining iron powder replacement and iron removal reagent treatment, the problems of low recovery rate and low electrolytic efficiency in the existing precious metal extraction methods are solved, and high-efficiency precious metal recycling and The recycling of copper trapping agents reduces costs and resource waste.
Patent Information
- Application Number
- CN202211409316.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-11
AI Technical Summary
Among the existing precious metal extraction methods, the wet process has low recovery rate and serious resource waste. The fire process requires the prerequisite for copper smelting. In the presence of iron, the electrolytic efficiency decreases, the power consumption increases, and the cost of trapping agent treatment is high.
The precious metal-containing material is mixed with copper and heated and melted in an arc furnace. After electrolytic separation, the cathode copper is cut and returned to melt. During the electrolysis process, part of the electrolyte is opened to remove iron. The iron ion concentration is reduced by replacing copper with iron powder and iron removal reagent. Copper trapping agent is recycled, and it has a wide range of applications that can handle iron-containing materials.
It improves the precious metal recovery rate, reduces the consumption and extraction cost of raw materials, realizes efficient recycling of precious metals and recycling of copper trapping agents, has a wide range of application and strong adaptability.
Smart Images

Figure CN115927869B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for extracting precious metals from precious metal-containing materials. Background Art
[0002] Some precious metal-containing materials, such as automobile exhaust waste catalysts, materials treated by wet methods, etc., contain precious metals such as Pt, Rh, Pd, etc. Currently, the methods for extracting precious metals include wet processes and pyroprocesses.
[0003] The wet process is to treat the material with an acid solution and then leach and separate it. The inventors of the present application realized that since the precious metals are in a state of existence or wrapped by a carrier, the direct use of wet recovery in this process leads to a very low recovery rate, resulting in a waste of resources. A certain factory used sulfuric acid and an oxidant to leach Pt-containing waste catalysts, and its leaching rate was only 95%, and the Pt content in the leached residue was still about 100g / t, resulting in a huge waste of Pt.
[0004] The pyrometallurgical process often uses collectors to capture precious metals, such as copper capture, but this usually requires the factory to have copper pyrometallurgical smelting as a prerequisite.
[0005] Some documents use copper capture-electrolysis process to extract precious metals. However, the inventors of the present application have found through research that the process still has limitations. It requires that there should be no iron in the processed raw materials. If the raw materials contain iron, a large amount of iron will enter the electrolyte during electrolysis, which will cause the electrolysis conditions to deteriorate, resulting in a sharp increase in power consumption, a sharp decrease in electrolysis efficiency, and even interruption of operation. In addition, the inventors of the present application also found that the current process also needs to provide a capture agent for capturing precious metals during the extraction process, and the processing cost is high. Based on the above findings and understandings, the inventors of the present application have provided a new method for extracting precious metals from precious metal-containing materials through further research and improvement. Summary of the invention
[0006] According to one embodiment of the present invention, an object is to provide a method for extracting precious metals from precious metal-containing materials.
[0007] The above purpose can be achieved by implementing the following technical solutions:
[0008] In one embodiment of the present invention, a method for extracting precious metals from precious metal-containing materials is provided, comprising: mixing the precious metal-containing material with copper, heating and smelting in an electric arc furnace, and separating slag from gold to obtain a precious metal-containing alloy; electrolyzing the precious metal-containing alloy to separate cathode copper and precious metal-containing anode mud, wherein during the electrolysis process, part of the electrolyte is opened to remove iron and the treated solution is returned to the electrolysis; the cathode copper is shredded and returned to smelting as copper, and the precious metal-containing anode mud is leached to obtain a precious metal solution.
[0009] Optionally, the open circuit amount is determined according to a control target that the iron ion concentration during the electrolysis process does not exceed 10 g / L.
[0010] Optionally, during the electrolysis process, the step of opening a circuit to remove iron from a portion of the electrolyte and returning the treated solution to the electrolysis includes sequentially performing copper replacement and iron removal. Further, the step includes: adding iron powder to the open-circuit electrolyte to replace copper, obtaining copper and a first solution, and returning the copper to smelting; adding an iron removal agent to the first solution to obtain a fourth solution, and returning the fourth solution to the electrolysis.
[0011] Optionally, during the electrolysis process, the step of opening a circuit to remove iron from a portion of the electrolyte and returning the treated solution to the electrolysis includes sequentially replacing copper, removing heavy metals, replacing copper again, and removing iron. Further, it includes: adding iron powder to the opened electrolyte to replace copper, obtaining copper and a first solution, and returning the copper to smelting; removing heavy metals from the first solution to obtain a second solution; adding iron powder to the second solution to replace copper again, obtaining copper and a third solution, and returning the copper to smelting; adding an iron removal agent to the third solution to obtain a fourth solution, and returning the fourth solution to the electrolysis.
[0012] Optionally, when iron powder is added to the open-circuit electrolyte to replace copper, the excess coefficient of iron powder is 1.05 to 2.5, and the copper ion concentration in the first solution is lower than 0.1 g / L.
[0013] Optionally, when the first solution is subjected to heavy metal removal treatment, sulfide is used to remove the heavy metal, and the sulfide excess coefficient is 1.05 to 3.0.
[0014] Optionally, when iron powder is added again to the second solution to replace copper, the end point pH of the solution is set to 4 to 4.8 to obtain a third solution.
[0015] Optionally, the iron removal agent is an alkaline agent, and the pH of the solution is adjusted to 7-8.5 to reduce the iron ion concentration in the fourth solution to below 0.1 g / L.
[0016] Optionally, the method further comprises: treating an alkali reagent to obtain an iron-containing precipitate, performing a polymerization reaction, and obtaining an iron-containing polymer; and using the iron-containing polymer as a water purifier.
[0017] Optionally, during heating and smelting, quenching treatment is performed when the temperature reaches a preset temperature, and slag-metal separation is performed after quenching treatment; wherein, the preset temperature is 1300° C. to 1500° C., and the holding time is 2 h to 6 h.
[0018] Optionally, the step of mixing the precious metal-containing material with copper and placing it in an electric arc furnace for heating and smelting includes: drying the precious metal-containing material and grinding it to a 200 mesh size of not less than 50%; mixing the ground precious metal-containing material with copper, adding auxiliary materials, and placing it in an electric arc furnace for heating and smelting.
[0019] Optionally, during mixing, the precious metal-containing material comprises 50 to 250 parts by mass and copper comprises 5 to 25 parts by mass.
[0020] Optionally, the auxiliary materials include, by weight: 10 to 20 parts by weight of calcium oxide, 10 to 20 parts by weight of silicon dioxide, 10 to 30 parts by weight of aluminum oxide, 5 to 20 parts by weight of boric acid, and 5 to 15 parts by weight of sodium carbonate.
[0021] According to one embodiment of the present invention, precious metal-containing materials and copper are placed in an electric arc furnace for heating and smelting. After smelting, the captured copper alloy (i.e., the precious metal-containing alloy) is cast into a copper electrode for electrolysis, and the precious metal enters the anode mud. After leaching treatment, a precious metal solution is obtained, and the cathode copper obtained by electrolytic separation is shredded and returned to the electric arc furnace for smelting. During the electrolysis process, iron is gradually enriched. By opening a circuit to discharge part of the electrolyte, the iron therein is removed and then returned for electrolysis, thereby reducing the iron ion concentration in the system, ensuring the stable operation of the electrolysis, and improving the recovery rate of precious metals. The method has a wide range of applications and strong raw material adaptability, and can especially process iron-containing materials. The method can process leached slag that has reached the limit of wet processing capacity; at the same time, the collector copper can be recycled, and it is not necessary for the factory to have a copper pyrometallurgical smelting production line, thereby reducing the consumption of raw copper and reducing the extraction cost.
[0022] Compared with the existing process, some embodiments of the present invention also have at least the following advantages and beneficial effects: 1) It has strong adaptability to raw materials and can process iron-containing materials. By opening part of the electrolyte, the electrolysis process can be operated stably. 2) Sponge copper is obtained by replacing the copper in the electrolyte opened by iron powder, and it is returned to smelting, and precious metals are captured based on the sponge copper; and / or, by crushing the cathode copper after electrolytic separation and returning it to smelting as copper, there is no need to continuously add copper during the extraction process, which greatly reduces the amount of raw copper used and reduces the cost of precious metal extraction. 3) The collector copper can be recycled, and iron is converted into ferrous hydroxide, which can be processed into a water purifier, realizing the full utilization of the main elements. 4) It can process wet-treated leaching residue, that is, it can process leaching residue that has reached the limit of wet treatment capacity, and has a wide range of uses. 5) The recovery rate of precious metals can be increased to more than 95%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention is a flowchart of a method for extracting precious metals from precious metal-containing materials in one embodiment of the present invention. DETAILED DESCRIPTION
[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] As described in the background technology, the inventors of the present application have found a series of problems existing in the prior art of precious metal extraction, especially the influence of the presence of iron in the raw material on the electrolytic process of extracting precious metals. For example, as long as the raw material contains iron, a large amount of iron will enter the electrolyte during electrolysis and continuously accumulate in the system, causing the electrolysis conditions to deteriorate, which has a serious impact on the electrolysis process, resulting in a sharp increase in power consumption and a sharp decrease in electrolysis efficiency, which seriously affects the electrolysis efficiency, deteriorates the operation of the electrolysis process, and even causes the operation to be interrupted. Through research and improvement, a new method for extracting precious metals from precious metal-containing materials is provided, which is to mix the precious metal-containing materials with copper and The alloy containing precious metals separated after smelting is heated and smelted in an electric arc furnace, and the precious metals enter the anode mud. The cathode copper separated by electrolysis is cut into pieces and returned to the electric arc furnace for smelting. During the electrolysis process, iron is gradually enriched, and part of the electrolyte is opened to remove the iron and then returned to the electrolysis system for electrolysis. The method ensures the stable operation of the electrolysis and improves the recovery rate of precious metals. The method has a wider range of applications. Since the iron is continuously opened, the method has no restrictions on whether the raw material contains iron and the specific iron content. Moreover, the copper collector can be recycled during the extraction process, which reduces the consumption of raw copper and reduces the extraction cost.
[0026] Figure 1 The process of extracting precious metals from precious metal-containing materials according to one embodiment of the present invention is schematically shown. Figure 1 As shown, the method for extracting precious metals from precious metal-containing materials comprises the following steps:
[0027] Step S10, mixing the precious metal-containing material, metallic copper and auxiliary materials, adding them into an electric arc furnace for heating and smelting, separating the slag and gold after smelting, and obtaining a precious metal-containing alloy and slag.
[0028] It should be noted that the precious metal-containing material is extracted by adding metallic copper. Of course, the precious metal-containing copper alloy and auxiliary materials can also be directly mixed and added to an electric arc furnace for heating and smelting. The specific type of material to be processed can be appropriately adjusted. Among them, the precious metal-containing material can be a precious metal-containing waste material to achieve waste utilization. The precious metal-containing material can be a leaching slag that has been treated by a wet method, that is, a leaching slag that has reached the limit capacity of the wet method. Especially for iron-containing materials, such as materials with an iron content of 3%, this method can ensure the stable operation of the electrolysis process of the material and achieve the beneficial effect of efficient extraction of precious metals.
[0029] In addition, the precious metal-containing material is dried before mixing, and then ground after drying, for example, it can be ground to -200 mesh accounting for 50%. By mixing the ground precious metal-containing material with metallic copper, and then adding auxiliary materials for mixed smelting, it is more conducive to the smelting process and improves the extraction efficiency of precious metals. Among them, the mass ratio of the precious metal-containing material and copper can be (50-250): (5-25); the auxiliary materials can be calcium oxide, silicon dioxide, borax, sodium carbonate and coke powder. Further, the material mixing ratio can be: 10-20 parts by mass of calcium oxide, 10-20 parts by mass of silicon dioxide, 10-30 parts by mass of aluminum oxide, 5-20 parts by mass of boric acid, 5-15 parts by mass of sodium carbonate, 5-25 parts of metallic copper, 50-250 parts by mass of precious metal-containing material. The above mixing ratio can further improve the smelting effect and the extraction efficiency of precious metals.
[0030] In addition, the mixed powder material is placed in an electric arc furnace for heating, and quenched when the temperature reaches a preset temperature, wherein the preset temperature is 1300°C to 1500°C, and the insulation time is 2h to 6h, to obtain a sample with a slag phase on the upper layer and a metal eutectic layer on the lower layer. The sample is subjected to slag / alloy separation to obtain a precious metal alloy and slag.
[0031] In this step, by optimizing the mass ratio of the raw materials and placing the mixed materials in an electric arc furnace for heating and melting while controlling the quenching temperature and time, the smelting process is more conducive to the enrichment of precious metals in the alloy to the greatest extent, thereby improving the extraction rate of precious metals.
[0032] Step S20, electrolyze the precious metal alloy separated after smelting, precious metal enters into anode mud, cathode copper and precious metal-containing anode mud are separated, cathode copper is cut into pieces and returned to the arc furnace as metal copper for heating and smelting, part of the electrolyte is opened during the electrolysis process and iron is removed before returning to electrolysis. Electrolyzing the precious metal alloy means casting the precious metal alloy (including copper) after smelting and capture into copper electrodes, electrolyzing, the cathode is an insoluble electrode, precious metal enters into anode mud, and cathode copper is obtained after separation.
[0033] The present application opens a portion of the electrolyte during the electrolysis process to reduce the Fe concentration in the electrolyte. The opening amount is determined based on process calculations, and the calculation basis and control target are to ensure that the iron concentration in the system does not exceed 10g / L. By opening a portion of the electrolyte according to the control target and removing iron from it before returning it to electrolysis, the iron concentration in the electrolyte of the electrolysis system is reduced and within the target range, ensuring the stable operation of the electrolysis process and improving the efficiency of precious metal extraction.
[0034] In an optional embodiment, the treatment of the open circuit electrolyte during the electrolysis process first replaces the copper and then removes the iron. Specifically includes:
[0035] 1) adding iron powder to the open-circuit electrolyte to replace copper, with an excess coefficient of iron powder of 1.05 to 2.5 (or making the solution end point pH 4 to 4.8) to ensure that copper can be completely replaced, to obtain sponge copper and a first solution, wherein the copper ion concentration in the first solution is reduced to below 0.1 g / L, and the sponge copper is returned to smelting as metallic copper, thereby reducing the loss of raw copper and allowing most of the copper to circulate in the system.
[0036] 2) Add a neutralizing agent, such as an alkaline agent, to the first solution, specifically, add sodium hydroxide, pass an oxygen-containing gas, adjust the final pH of the solution to 7-8.5, at which time the Fe concentration in the solution is reduced to below 0.1 g / L, obtain a fourth solution, and return the fourth solution to electrolysis, thereby reducing the iron concentration in the electrolyte of the electrolysis system, ensuring the stable operation of the electrolysis process. By controlling the pH of the solution after iron removal to between 7 and 8.5 and passing air or oxygen, most of the iron in the solution can be neutralized and precipitated. If it is not within this range, there will be problems of incomplete precipitation of iron or excessive neutralizer.
[0037] In an optional embodiment, the treatment of the open circuit electrolyte during the electrolysis process sequentially replaces copper, removes heavy metals, replaces copper again, and removes iron. Specifically, it includes:
[0038] 1) adding iron powder to the open-circuit electrolyte to replace copper, with an excess coefficient of iron powder of 1.05 to 2.5, to ensure that copper can be completely replaced, to obtain sponge copper and a first solution, wherein the copper ion concentration in the first solution is reduced to below 0.1 g / L, and the sponge copper is returned to smelting as metallic copper, thereby reducing the loss of raw copper and allowing most of the copper to circulate in the system.
[0039] 2) adding sulfide to the first solution to remove heavy metals, wherein the excess coefficient of sulfide is 1.05 to 3.0 to ensure that the heavy metals are completely removed, and obtaining a second solution.
[0040] 3) Add iron powder to the second solution again to replace copper, so that the solution end point pH is 4 to 4.8, and after a reaction time of 1 to 3 hours, the Cu concentration in the solution is lower than 0.1 g / L, and a third solution is obtained, and the sponge copper obtained by replacement is also returned to smelting as metallic copper. By adding iron powder to replace copper again after removing heavy metals and returning the sponge copper to smelting, the recycling of the collector copper can be further achieved; at the same time, by continuing to control the pH between 4 and 4.8 after adding iron powder again, it can be ensured that most of the copper in the solution is precipitated. If it is not within this range, there will be problems of incomplete copper recovery or excessive iron powder.
[0041] 4) Use a neutralization method to remove iron from the third solution. Specifically, add a neutralizing agent, such as an alkaline agent, to the third solution, specifically, add sodium hydroxide, adjust the final pH of the solution to 7-8.5, at which time the Fe concentration in the solution is reduced to below 0.1 g / L, obtain a fourth solution, and return the fourth solution to electrolysis, thereby reducing the iron concentration in the electrolyte of the electrolysis system, ensuring the stable operation of the electrolysis process. By controlling the pH of the solution after iron removal to between 7 and 8.5 and passing air or oxygen, most of the iron in the solution can be neutralized and precipitated. If it is not within this range, there will be problems of incomplete precipitation of iron or excessive neutralizer.
[0042] Step S30, wet leaching is performed on the anode mud containing precious metals to obtain leached residue and precious metal solution containing main precious metals. The precious metal solution can be further separated from each precious metal by existing technology, which is not specifically limited.
[0043] In addition, the method for extracting precious metals from precious metal-containing materials may further include step S40, collecting iron and applying it. For example, the iron is converted into ferrous hydroxide and / or ferric hydroxide by a neutralization and iron removal method, and then used as a water purifier after processing, thereby achieving full utilization of important elements in the extraction process.
[0044] In some embodiments of the present invention, the pyrometallurgical method and the hydrometallurgical method are combined to extract and recover precious metals. Copper is used to capture precious metals, and the captured copper alloy is cast into copper electrodes for electrolysis, and the precious metals enter the anode mud. The electrolyte is open-circuited to remove iron from the electrolyte and return it to the electrolysis, thereby reducing the iron concentration in the electrolyte and ensuring the stable operation of the electrolysis system. The recovery rate of precious metals is increased to more than 95%, and the method has strong adaptability to raw material processing and can process iron-containing materials. At the same time, the sponge copper obtained by electrolytic separation of cathode copper and / or open-circuit treatment is circulated in the system, without the need for the factory to have a copper pyrometallurgical smelting production line, thereby reducing the consumption of raw copper.
[0045] The following is a further description of the implementation of the present invention in conjunction with a specific embodiment and its effects:
[0046] Embodiment 1:
[0047] The composition of precious metal-containing materials is shown in Table 1 below:
[0048] Table 1 Composition of precious metal-containing materials
[0049] element Pt Pd Fe Al Si content(%) 0.122 0.0145 10.52 20.86 14.43
[0050] The raw materials were crushed to -200 mesh, accounting for 50%, and 100 kg was taken. 15 kg CaO, 20 kg SiO2, 20 kg Al2O3, 5 kg boric acid, 5 kg Na2CO3, and 15 kg sponge copper were mixed and placed in an electric arc furnace and heated to 1350°C. The mixture was kept warm for 3 hours, and the lower copper alloy (i.e., the alloy containing precious metals) was taken out. The composition is shown in Table 2 below:
[0051] Table 2 Alloy composition
[0052] element Pt Pd Fe Al Si content(%) 8.32 0.16 7.71 1.07 -
[0053] The copper alloy was processed into electrodes for electrolysis, and a titanium plate of the same size was used as the cathode. After 48 hours of electrolysis, the Fe concentration in the solution increased to 18 g / L, at which time the anode electrolysis efficiency was reduced to 50%. Half of the electrolyte was taken out for treatment. The specific treatment method is: add iron powder while stirring, react to pH 4.4, at which time the Cu concentration in the solution is lower than the detection limit (i.e. 0.1 g / L), and then pass air into the stirring solution at a rate of 1 L / (min·L solution), and at the same time add NaOH to adjust the solution pH to 8.0, at which time the Fe concentration in the solution is lower than the detection limit (i.e. 0.1 g / L). The treated solution is returned to the electrolyte, and the iron ion concentration in the solution is reduced to 9 g / L, at which time the anode electrolysis efficiency is increased to 90%.
[0054] The copper obtained by replacing iron can be used for processing precious metal copper alloys. The precipitated iron hydroxide can be converted into polyferric sulfate by adding sulfuric acid, oxygen and sodium nitrite to the reactor for polymerization catalysis, and the polyferric sulfate can be used as a water purifier.
[0055] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.
Claims
1. A method for extracting precious metals from precious metal-containing materials, characterized in that: include: The precious metal-containing material is mixed with copper, and heated and smelted in an electric arc furnace, and the slag and gold are separated to obtain a precious metal-containing alloy; wherein the precious metal-containing material contains iron; The precious metal alloy is electrolyzed to separate cathode copper and precious metal-containing anode mud; during the electrolysis process, part of the electrolyte is opened for iron removal and the treated solution is returned to the electrolysis process; the open circuit amount is determined according to the control target that the iron ion concentration during the electrolysis process does not exceed 10g / L; the cathode copper is cut into pieces and returned to smelting as copper, and the precious metal-containing anode mud is leached to obtain a precious metal solution; The method of opening a circuit to remove iron from a portion of the electrolyte during the electrolysis process refers to: sequentially replacing copper and removing iron; or sequentially replacing copper, removing heavy metals, replacing copper again, and removing iron; wherein the copper is replaced by iron powder, and the replaced copper is returned to smelting; the iron powder excess coefficient is 1.05 to 2.5, and the copper ion concentration in the solution after the copper is replaced is less than 0.1 g / L.
2. The method for extracting precious metals from precious metal-containing materials according to claim 1, characterized in that: During the electrolysis process, a portion of the electrolyte is opened to sequentially replace copper and remove iron, and the treated solution is returned to the electrolysis step, including: Adding iron powder to the electrolyte discharged from the open circuit to replace copper, obtaining copper and a first solution, and returning the copper to smelting; An iron removal agent is added to the first solution to obtain a fourth solution, and the fourth solution is returned to electrolysis.
3. The method for extracting precious metals from precious metal-containing materials according to claim 1, characterized in that: During the electrolysis process, a portion of the electrolyte is opened to sequentially replace copper, remove heavy metals, replace copper again, and remove iron, and the treated solution is returned to the electrolysis step, including: Adding iron powder to the electrolyte discharged from the open circuit to replace copper, obtaining copper and a first solution, and returning the copper to smelting; performing heavy metal removal treatment on the first solution to obtain a second solution; Adding iron powder to the second solution again to replace copper, obtaining copper and a third solution, and returning the copper to smelting; An iron removal agent is added to the third solution to obtain a fourth solution, and the fourth solution is returned to electrolysis.
4. The method for extracting precious metals from precious metal-containing materials according to claim 3, characterized in that: When the first solution is subjected to heavy metal removal treatment, sulfide is used to remove the heavy metal, and the excess coefficient of sulfide is 1.05 to 3.
0.
5. The method for extracting precious metals from precious metal-containing materials according to claim 3, characterized in that: When iron powder is added again to the second solution to replace copper, the end point pH of the solution is adjusted to 4 to 4.8 to obtain a third solution.
6. The method for extracting precious metals from precious metal-containing materials according to claim 2 or 3, characterized in that: The iron removal reagent is an alkaline reagent, and the pH of the solution is adjusted to 7-8.5 to reduce the iron ion concentration in the solution to below 0.1 g / L.
7. The method for extracting precious metals from precious metal-containing materials according to claim 6, characterized in that: Also includes: The iron-containing precipitate is treated with an alkali reagent and subjected to polymerization reaction to obtain an iron-containing polymer; The iron-containing polymer is used as a water purifier.
8. The method for extracting precious metals from precious metal-containing materials according to claim 1, characterized in that: During heating and smelting, when the temperature reaches a preset temperature, quenching treatment is performed, and slag-metal separation is performed after quenching treatment; wherein, the preset temperature is 1300° C. to 1500° C., and the holding time is 2h to 6h.
9. The method for extracting precious metals from precious metal-containing materials according to claim 1, characterized in that: The steps of mixing precious metal-containing materials with copper and heating and smelting them in an electric arc furnace include: Drying the precious metal-containing material and grinding it to a 200-mesh size of not less than 50%; The ground precious metal-containing material is mixed with copper, and auxiliary materials are added to heat and melt in an electric arc furnace.
10. The method for extracting precious metals from precious metal-containing materials according to claim 9, characterized in that: When mixed, the precious metal-containing material is 50 to 250 parts by mass, and copper is 5 to 25 parts; And / or, the auxiliary materials include, by weight: 10 to 20 parts by weight of calcium oxide, 10 to 20 parts by weight of silicon dioxide, 10 to 30 parts by weight of aluminum oxide, 5 to 20 parts by weight of boric acid, and 5 to 15 parts by weight of sodium carbonate.