Preparation method of nano-homogenized TiB2 in-situ reinforced aluminum-based composite material
By mixing the fluorine salt in a specific proportion in the aluminum-based composite material and remelting it in an intermediate frequency furnace, combining graphite rod rotating mechanical stirring and internal cooling system pouring, the problem of poor melt uniformity of TiB2 in-situ enhanced aluminum-based composite material is solved. , realizes nano-uniformization of TiB2 phase, improves material performance and simplifies production process.
Patent Information
- Application Number
- CN202211600698.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-13
AI Technical Summary
The existing preparation methods of TiB2 in-situ reinforced aluminum-based composites are difficult to achieve the integrated treatment of the melt, resulting in poor uniformity of the melt, and the generated TiB2 phase is prone to agglomeration, which fails to fully exert the nano-enhancement effect.
By mixing the fluorine salts K2TiF6 and KBF4 at a ratio of 1:2 to Ti:B, adding pure aluminum melt to react to produce TiB2, using medium-frequency furnace remelting and graphite rod rotary mechanical stirring, combined with the internal cooling system Gravity casting system realizes nano-uniformization of TiB2 phase.
The nano-uniformization of the TiB2 phase is achieved, agglomeration is avoided, the strength and elastic modulus of the material are improved, the process flow is simplified, the cost is reduced, and it is suitable for engineering production.
Smart Images

Figure CN115927902B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal composite materials and relates to a method for preparing a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material. Background Art
[0002] Aluminum-based composite materials have become a research hotspot for new structural functional materials due to their light weight, high specific strength, high specific modulus, and strong design performance. According to the different ways of reinforcing the matrix, aluminum-based composite materials can be divided into externally reinforced aluminum-based composite materials and in-situ reinforced aluminum-based composite materials. In the in-situ reinforced aluminum-based composite material series, the TiB2 phase has good stability and a good contact interface with the aluminum matrix. At the same time, the TiB2 phase has a coherent relationship with the aluminum alloy matrix and can serve as an effective nucleation substrate, playing a role in heterogeneous nucleation and grain refinement, significantly improving the strength, toughness and elastic modulus of the material. Therefore, TiB2 in-situ reinforced aluminum-based composite materials have very broad application prospects in military and civilian fields such as aviation, aerospace, shipbuilding, and transportation.
[0003] At present, the engineering preparation method of TiB2 in-situ reinforced aluminum-based composite materials is mainly the fluoride salt method, in which fluoride salts containing Ti and B elements are added to the aluminum alloy melt to generate TiB2 phase through in-situ reaction to prepare aluminum-based composite materials. Since the TiB2 phase generated by the in-situ reaction is generally nanoscale and has high surface activity, it is easy to agglomerate in the aluminum-based composite material. The TiB2 clusters generated by agglomeration are more than ten microns or even tens of microns in size, and the strengthening effect of the nano-reinforcement of TiB2 itself on the matrix is not fully exerted; in addition, since a large amount of fluoride salts are introduced during the material preparation process, how to effectively remove the residual products has also become an important factor in ensuring the excellent comprehensive performance of the material.
[0004] In response to the above problems, Patent 110257655A reports a highly dispersed nano-titanium diboride particle reinforced aluminum-based composite material and its preparation method. The patent uses ultrasonic stirring to treat the melt, and then pours it into a mold. During its solidification process, ultrasound is applied (introduced through the bottom introduction method) to obtain a dispersed nano-TiB2 particle reinforced aluminum-based composite material. In this method, the area affected by ultrasound on the melt solidification process is limited, and the overall treatment of the melt cannot be achieved, making it difficult to ensure the consistent uniformity of the melt. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material, which solves the problem that the existing method is difficult to achieve integrated processing of the melt, resulting in poor uniformity of the melt.
[0006] The technical solution adopted by the present invention is a method for preparing a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material, comprising the following steps:
[0007] Step 1: Evenly mix the fluoride salts K2TiF6 and KBF4, and then add them into the pure aluminum melt to react and generate a TiB2 in-situ reinforced aluminum-based composite material melt, and cast to obtain a precast ingot with a thickness of 10 mm to 20 mm;
[0008] Step 2: placing the precast ingot obtained in step 1 into a medium frequency induction furnace, heating and melting it, and performing classification treatment on the melt to obtain a nano-homogenized melt;
[0009] Step 3: pouring the melt through a gravity pouring system with an internal cooling system to obtain a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material, wherein the mass ratio of TiB2 is 8%-12%.
[0010] In step 1, fluoride salts K2TiF6 and KBF4 are mixed in a ratio of Ti:B of 1:2.
[0011] In step 1, the fluoride salts K2TiF6 and KBF4 are mixed evenly in a ball mill and placed in a drying oven for later use.
[0012] In step 1, the temperature of the pure aluminum melt is 810°C-850°C.
[0013] In step 1, the evenly mixed fluoride salt is added to the pure aluminum melt in 3 to 5 times, and each time the mixture is allowed to stand for 10 to 20 minutes. The upper reaction product is then skimmed off, the melt is stirred, and a precast ingot is obtained by pouring the mixture into a metal ingot mold.
[0014] In step 2, the melt is graded, including first controlling the melt at 760-800°C, refining the melt by blowing argon with a rotating graphite rod, then skimming off the slag, heating the melt to 910-950°C, and mechanically stirring the melt with a rotating graphite rod.
[0015] In step 2, a graphite rod is used to rotate and argon is blown to refine the melt for 30 to 40 minutes, and the rotation speed of the graphite rod is 300 to 400 r / min.
[0016] In step 2, a graphite rod is used to rotate the melt for 20 to 30 minutes, and the rotation speed of the graphite rod is 600 to 700 r / min.
[0017] The gravity pouring system with internal cooling system is a metal mold flow curve gravity pouring system.
[0018] The beneficial effects of the present invention are that the fluorine salts K2TiF6 and KBF4 are uniformly mixed and added to the pure aluminum melt, thereby ensuring the continuity and sufficiency of the TiB2 in-situ autogenous reaction process; casting a thin precast ingot with a thickness of 10 mm to 20 mm can make the TiB2 phase generated in the melt solidify uniformly in the precast ingot, thereby avoiding the TiB2 phase from being pushed and aggregated during sequential solidification of the thick ingot; using a medium frequency furnace to remelt the precast ingot is conducive to the homogenization of the TiB2 phase during movement; at the same time, under the multiple effects of the electromagnetic field and the graphite rod rotating mechanical stirring, the TiB2 clusters undergo irreversible transformation, thereby realizing the nano-homogenization of the TiB2 phase; using a cooling water system The metal flow curve-shaped gravity casting system is used to cast the TiB2 in-situ reinforced aluminum-based composite material melt. A large number of crystal nuclei are formed at the contact interface between the highly superheated melt and the water-cooled metal mold wall, and are evenly dispersed into the melt during the flow process, which plays a positive role in the refinement of α-Al and the uniform distribution of TiB2 phase, and improves the phenomenon that the TiB2 phase is concentratedly pushed by the liquid / solid interface front during the solidification process, resulting in macroscopic agglomeration of the TiB2 phase. The equipment used in the melt treatment process of this achievement are all industrial standard equipment, and the auxiliary tooling and molds are simple in structure and low in cost. There is no special equipment such as electromagnetic and ultrasonic equipment, which can realize the engineering production of aluminum-based composite materials and their products. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a structural schematic diagram of a gravity pouring system with an internal cooling system in the present invention;
[0020] Figure 2 This is a metallographic diagram of the nano-homogenized TiB2 in-situ reinforced aluminum-based composite material prepared in Embodiment 1 of the present invention;
[0021] Figure 3 It is a metallographic diagram of TiB2 in-situ reinforced aluminum-based composite material prepared by existing methods.
[0022] In the figure, 1. metal mold shell, 2. internal cooling system, 3. flow curve gravity pouring system, 31. gate pool, 32. straight runner, 33. runner transition arc, 34. horizontal runner, 35. gate. DETAILED DESCRIPTION
[0023] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0024] A method for preparing a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material comprises the following steps:
[0025] Step 1: Preparing a precast ingot
[0026] Step 1.1, weighing fluoride salts K2TiF6 and KBF4 in a ratio of Ti:B of 1:2, mixing the fluoride salts K2TiF6 and KBF4 in a ball mill, and placing them in a drying oven for later use;
[0027] Step 1.2, melting the pure aluminum ingot, controlling the temperature of the pure aluminum melt at 810°C-850°C, then adding the mixed fluoride salt in the drying oven to the pure aluminum melt in 3-5 times, standing for 10-20 minutes after each addition, skimming off the upper layer of reaction products, stirring the melt, and finally reacting to generate a TiB2 in-situ reinforced aluminum-based composite melt;
[0028] Step 1.3, pouring the melt into a metal ingot mold to obtain a TiB2 in-situ reinforced aluminum-based composite precast ingot with a thickness of 10 mm to 20 mm;
[0029] During the in-situ autogenous process of TiB2 phase, the mixed fluoride salt is added in 3 to 5 times, and each time it is added, it is left to stand for 10 to 20 minutes. This treatment ensures that the composite fluoride salt can fully contact and react with the aluminum melt. TiB2 is continuously generated at the contact interface between the upper aluminum melt and the composite fluoride salt, and gradually settles into the lower aluminum melt. After the single reaction is completed, new composite fluoride salt is added. This ensures the continuity and sufficiency of the in-situ autogenous reaction process of TiB2, and avoids the phenomenon of salt slag being easily mixed in the melt during the conventional one-time addition of fluoride salt and auxiliary stirring. After the completion of all reactions and the removal of the upper reaction products, the melt is stirred again. At the same time, a thin precast ingot with a thickness of 10 to 20 mm is required to be cast in a metal ingot mold. The advantage of this treatment is that the TiB2 phase generated in the melt can be evenly solidified in the precast ingot, avoiding the phenomenon of TiB2 phase being pushed and aggregated during sequential solidification of large thickness ingots.
[0030] Step 2: Preparation of nano-homogenized melt
[0031] Step 2.1, the precast ingot obtained in step 1 is loaded into a medium frequency induction furnace, heated and melted, the melt temperature is maintained at 760-800° C., the melt is refined by argon blowing with a rotating graphite rod for 30-40 minutes, the rotation speed of the graphite rod is 300-400 r / min, and then the slag is skimmed off;
[0032] Step 2.2, heating the melt to 910-950° C., mechanically stirring the melt with a graphite rod for 20-30 minutes, the graphite rod rotating at a speed of 600-700 r / min, and then skimming off the slag to obtain a nano-homogenized melt;
[0033] The precast ingot is remelted in a medium frequency furnace, and the fast melting speed and high melting temperature of the medium frequency furnace and the stirring and disturbance function of the electromagnetic field on the melt are utilized, which is beneficial to the homogenization of the TiB2 phase during movement; at 760-800℃, the graphite rod rotates at a low speed and the melt is refined by rotating argon gas injection, the main purpose of which is to fully remove the residual slag, salt slag, etc. in the melt; at 910-950℃, the melt is overheated and rotated at a high speed, the main purpose of which is to fully decompose, crush and refine the micron-sized TiB2 clusters in the melt, and at the same time, under the multiple effects of the electromagnetic field and the mechanical stirring of the rotating graphite rod, the TiB2 clusters undergo irreversible transformation, thereby realizing the nano-homogenization of the TiB2 phase.
[0034] Step 3: Prepare the composite material
[0035] Step 3.1, refer to Figure 1 , prepare a metal mold flow curve-shaped gravity pouring system with an internal cooling system, including a metal mold shell 1, in which an internal cooling system 2 and a flow curve-shaped gravity pouring system 3 are arranged. In this embodiment, the internal cooling system 2 is a water cooling system, i.e., a water cooling channel. The flow curve-shaped gravity pouring system 3 is as described in the applicant's patent ZL201911221264.9, and includes a gate pool 31, a sprue 32 and a runner 34 arranged in sequence from top to bottom. The sprue 32 and the runner 34 are transitionally connected by a runner transition arc 33, and a gate 35 is arranged at the outlet of the runner 34;
[0036] The benefit of using a metal flow curve shaped gravity casting system with a cooling water system to cast the TiB2 in-situ reinforced aluminum-based composite material melt is that when the melt passes through the flow curve shaped gravity casting system, there is no gas gap between the melt and the casting system wall, and a large number of crystal nuclei are formed at the contact interface between the highly superheated melt and the water-cooled metal mold wall, and are evenly dispersed into the melt during the flow process, which plays a positive role in the refinement of α-Al and the uniform distribution of the TiB2 phase, and improves the phenomenon that the TiB2 phase is concentratedly pushed by the liquid / solid interface front during the solidification process, thereby leading to macroscopic agglomeration of the TiB2 phase.
[0037] Step 3.2, pouring the nano-homogenized melt through the pouring system in step 3.1 to obtain a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material, wherein the mass ratio of TiB2 is 8%-12%.
[0038] Example 1
[0039] A method for preparing a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material comprises the following steps:
[0040] Step 1: Preparing a precast ingot
[0041] Step 1.1, according to the atomic ratio of Ti:B being 1:2, weigh 2kg of K2TiF6 fluoride salt, 2.09kg of KBF4 fluoride salt, and 6.65kg of pure aluminum, mix the fluoride salt K2TiF6 and KBF4 in a ball mill evenly, and place them in a drying oven for later use;
[0042] Step 1.2, melt the weighed pure aluminum ingot, control the temperature of the pure aluminum melt at 810°C, then add the mixed fluoride salt in the drying oven to the pure aluminum melt three times, let it stand for 10 minutes after each addition, skim off the upper layer of reaction products, stir the melt, and finally react to generate a TiB2 in-situ reinforced aluminum-based composite melt;
[0043] Step 1.3, pouring the melt into a metal ingot mold to obtain a 10 mm thick TiB2 in-situ reinforced aluminum-based composite precast ingot;
[0044] Step 2: Preparation of nano-homogenized melt
[0045] Step 2.1, the precast ingot obtained in step 1 is loaded into a medium frequency induction furnace, heated and melted, the melt temperature is maintained at 760°C, and the melt is refined for 30 minutes by rotating a graphite rod and blowing argon gas, the rotation speed of the graphite rod is 300r / min, and then the slag is skimmed off;
[0046] Step 2.2, heating the melt to 910° C., stirring the melt for 20 min using a graphite rod rotating machine, the graphite rod rotating speed being 600 r / min, and then skimming off the slag to obtain a nano-homogenized melt;
[0047] Step 3: Preparation of composite materials
[0048] Step 3.1, prepare a metal mold flow curve gravity pouring system with a water cooling system for standby use, the flow curve gravity pouring system is as described in the applicant's patent ZL201911221264.9;
[0049] Step 3.2, pouring the nano-homogenized melt through the pouring system in step 3.1 to obtain a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material, wherein the mass ratio of TiB2 is 8%.
[0050] The microstructure of the prepared nano-homogenized TiB2 in-situ reinforced aluminum matrix composite material was observed, and its metallographic image is shown in Figure 2 As shown, Figure 3 The metallographic diagram of TiB2 in-situ reinforced aluminum matrix composite prepared by the existing method is shown in Figure 2. Figure 2 and Figure 3By comparison, it can be seen that the TiB2 particles in the TiB2 in-situ reinforced aluminum-based composite material prepared by the existing method have a larger particle size and obvious agglomeration, while the TiB2 particles in the TiB2 in-situ reinforced aluminum-based composite material prepared by the method of the present invention have a smaller particle size and are more evenly distributed.
[0051] Example 2
[0052] A method for preparing a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material comprises the following steps:
[0053] Step 1: Preparing a precast ingot
[0054] Step 1.1, according to the atomic ratio of Ti:B being 1:2, weigh 2kg of K2TiF6 fluoride salt, 2.09kg of KBF4 fluoride salt, and 5kg of pure aluminum, mix the fluoride salt K2TiF6 and KBF4 in a ball mill evenly, and place them in a drying oven for later use;
[0055] Step 1.2, melt the weighed pure aluminum ingot, control the temperature of the pure aluminum melt at 830°C, then add the mixed fluoride salt in the drying oven into the pure aluminum melt four times, let it stand for 15 minutes after each addition, skim off the upper layer of reaction products, stir the melt, and finally react to generate a TiB2 in-situ reinforced aluminum-based composite melt;
[0056] Step 1.3, pouring the melt into a metal ingot mold to obtain a 15 mm thick TiB2 in-situ reinforced aluminum-based composite precast ingot;
[0057] Step 2: Preparation of nano-homogenized melt
[0058] Step 2.1, the precast ingot obtained in step 1 is loaded into a medium frequency induction furnace, heated and melted, the melt temperature is maintained at 780°C, and the melt is refined for 35 minutes by using a graphite rod to rotate argon gas, the graphite rod rotation speed is 350r / min, and then the slag is skimmed off;
[0059] Step 2.2, heating the melt to 930° C., stirring the melt for 25 min using a graphite rod rotating machine, the graphite rod rotating speed being 650 r / min, and then skimming off the slag to obtain a nano-homogenized melt;
[0060] Step 3: Preparation of composite materials
[0061] Step 3.1, prepare a metal mold flow curve gravity pouring system with a water cooling system for standby use, the flow curve gravity pouring system is as described in the applicant's patent ZL201911221264.9;
[0062] Step 3.2, pouring the nano-homogenized melt through the pouring system in step 3.1 to obtain a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material, wherein the mass ratio of TiB2 is 10%.
[0063] Example 3
[0064] A method for preparing a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material comprises the following steps:
[0065] Step 1: Preparing a precast ingot
[0066] Step 1.1, according to the atomic ratio of Ti:B being 1:2, weigh 2kg of K2TiF6 fluoride salt, 2.09kg of KBF4 fluoride salt, and 4.25kg of pure aluminum, mix the fluoride salt K2TiF6 and KBF4 in a ball mill evenly, and place them in a drying oven for later use;
[0067] Step 1.2, melt the weighed pure aluminum ingot, control the temperature of the pure aluminum melt at 850°C, then add the mixed fluoride salt in the drying oven to the pure aluminum melt in 5 times, let it stand for 20 minutes after each addition, skim off the upper layer of reaction products, stir the melt, and finally react to generate a TiB2 in-situ reinforced aluminum-based composite melt;
[0068] Step 1.3, pouring the melt into a metal ingot mold to obtain a 20 mm thick TiB2 in-situ reinforced aluminum-based composite precast ingot;
[0069] Step 2: Preparation of nano-homogenized melt
[0070] Step 2.1, the precast ingot obtained in step 1 is loaded into a medium frequency induction furnace, heated and melted, the melt temperature is maintained at 800°C, and the melt is refined by argon blowing with a graphite rod rotating for 40 minutes, the graphite rod rotating speed is 400r / min, and then the slag is skimmed off;
[0071] Step 2.2, heating the melt to 950° C., using a graphite rod to mechanically stir the melt for 30 minutes, the graphite rod rotating speed being 700 r / min, and then skimming off the slag to obtain a nano-homogenized melt;
[0072] Step 3: Preparation of composite materials
[0073] Step 3.1, prepare a metal mold flow curve gravity pouring system with a water cooling system for standby use, the flow curve gravity pouring system is as described in the applicant's patent ZL201911221264.9;
[0074] Step 3.2, pouring the nano-homogenized melt through the pouring system in step 3.1 to obtain a nano-homogenized TiB2 in-situ reinforced aluminum-based composite material, wherein the mass ratio of TiB2 is 12%.
Claims
1. Nano-homogenized TiB 2 Preparation method of in-situ reinforced aluminum-based composite material, It is characterized in that The following steps are involved: Step 1: Add fluoride salt K 2 TiF 6 and KBF 4 Mix them evenly in a ball mill according to the atomic ratio of Ti:B of 1:2, place them in a drying oven for later use, and then add them into pure aluminum melt at a temperature of 810℃-850℃ to react and generate TiB 2 In-situ reinforced aluminum matrix composite material melt, casting to obtain a precast ingot with a thickness of 10 to 20 mm; Step 2: placing the precast ingot obtained in step 1 into a medium frequency induction furnace, heating and melting it, and performing classification treatment on the melt to obtain a nano-homogenized melt; In the step 2, the melt is subjected to a graded treatment, including first controlling the melt at 760-800° C., refining the melt by blowing argon gas with a graphite rod, then skimming off the slag, heating the melt to 910-950° C., and mechanically stirring the melt with a graphite rod; The melt is refined by argon blowing with a rotating graphite rod for 30 to 40 minutes, and the rotation speed of the graphite rod is 300 to 400 r / min; The melt is stirred for 20 to 30 minutes using a graphite rod rotating machine, and the graphite rod rotating speed is 600 to 700 r / min; Step 3: pouring the melt through a gravity pouring system with an internal cooling system, wherein the gravity pouring system with an internal cooling system is a metal mold flow curve-shaped gravity pouring system, to obtain nano-homogenized TiB 2 In-situ reinforced aluminum matrix composites, in which TiB 2 The mass ratio is 8%-12%.
2. The nano-homogenized TiB according to claim 1 2 Preparation method of in-situ reinforced aluminum-based composite material, It is characterized in that In the step 1, the evenly mixed fluoride salt is added to the pure aluminum melt in 3 to 5 times, and the mixture is allowed to stand for 10 to 20 minutes after each addition. Then, the upper reaction product is skimmed off, the melt is stirred, and the precast ingot is cast in a metal ingot mold.