A high-temperature self-lubricating periodic multilayer structure coating and preparation method thereof

By using (CrNbTiAlV) CNx/MoN multi-layer structural coatings with different modulation periods, the problem of poor lubrication performance of aero-engine bearings in high-temperature environments is solved, and a high-temperature self-lubricating effect of low friction coefficient and high bonding force is achieved.

CN115928019BActive Publication Date: 2024-10-29LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211509456.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2024-10-29
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

It is difficult for aircraft engine bearings to achieve wear-resistant lubrication in high-temperature environments. The single-structure high-entropy nitride coating has a high friction coefficient and poor oxidation resistance. It is difficult for existing technology to effectively synergize the strength and lubrication performance of the coating at high temperatures.

Method used

Through the (CrNbTiAlV) CNx/MoN multi-layer structure coating with different modulation periods, the Cr bonding layer and the alternately deposited (CrNbTiAlV) CNx/MoN layer are deposited using magnetron sputtering technology. The modulation period is 50~420 nm, and the modulation ratio is 1:1~1.2:1, forming a coating with high temperature self-lubricating properties.

Benefits of technology

At 500°C, the friction coefficient is reduced to 0.11~0.34, and the bonding force between the coating and the substrate is 65~85 N, achieving the lowest friction coefficient and good self-lubricating performance in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115928019B_ABST
    Figure CN115928019B_ABST
Patent Text Reader

Abstract

The present invention relates to a high-temperature self-lubricating periodic multilayer structure coating, which comprises a substrate, a Cr bonding layer and (CrNbTiAlV)CN sequentially deposited on the outer surface of the substrate. x / MoN top layer composition; the (CrNbTiAlV)CN x / MoN top layer is composed of (CrNbTiAlV)CN x The invention also discloses a method for preparing the periodic multilayer structure coating. The invention adopts magnetron sputtering technology to prepare (CrNbTiAlV)CN with different modulation periods by changing the deposition time of the single-layer coating. x / MoN multilayer structure coating; prepared (CrNbTiAlV)CN x The MoN / MoN multilayer composite coating has a smooth interface between layers, a clear and dense periodic structure, and good self-lubricating properties at high temperatures. It can be used for friction-reducing and wear-resistant parts in high temperature environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of bearing surface protection, and in particular to a coating with a high-temperature self-lubricating periodic multilayer structure and a preparation method thereof. Background Art

[0002] As the new generation of aircraft engines are developing towards a high thrust-to-weight ratio, high durability and low fuel consumption, the bearings serving in aircraft engines are facing complex and harsh working conditions such as heavy load, high speed and oil cut-off. Therefore, the development of new high-temperature resistant, high-load, low-friction and wear-resistant solid lubricating coating materials is of great significance to breaking through the bottleneck of lubrication performance between key mechanical moving parts.

[0003] Hard high entropy nitride coatings have high load-bearing capacity, can reduce abrasive wear and extend friction life, but single-structure high entropy nitride coatings have high friction coefficients and poor oxidation resistance at high temperatures. MoN coatings have good high-temperature lubrication properties and form easily sheared MoO 3 Lubricating phase. Constructing a nano multilayer structure can achieve effective synergy between the strength and lubrication performance of the coating. Therefore, by regulating the periodic thickness of the hard high entropy nitride coating and the MoN coating, the effective synergistic lubrication effect between the two coatings at high temperatures is fully utilized to solve the technical problem of high-temperature wear-resistant lubricating coatings for aircraft engine bearings. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a high-temperature self-lubricating periodic multilayer structure coating with different modulation periods.

[0005] Another technical problem to be solved by the present invention is to provide a method for preparing the coating with high-temperature self-lubricating periodic multi-layer structure.

[0006] In order to solve the above problems, the present invention discloses a high-temperature self-lubricating periodic multilayer structure coating, characterized in that the periodic multilayer structure coating comprises a substrate, a Cr bonding layer and (CrNbTiAlV)CN sequentially deposited on the outer surface of the substrate. x / MoN top layer composition; the (CrNbTiAlV)CN x / MoN top layer is composed of (CrNbTiAlV)CN x The modulation period is 50~420 nm and the modulation ratio is 1:1~1.2:1.

[0007] The method for preparing the high-temperature self-lubricating periodic multilayer structure coating as described above comprises the following steps:

[0008] ⑴Pretreat the substrate;

[0009] (2) Place the pretreated substrate into a vacuum chamber for evacuation. When the vacuum degree is lower than 1×10 -3 When Pa, the substrate surface is sputter-cleaned by bombarding the substrate with ions to obtain a cleaned substrate;

[0010] ⑶ Using magnetron sputtering technology, a Cr bonding layer is first deposited on the surface of the cleaned substrate, and then (CrNbTiAlV)CN is alternately deposited by magnetron sputtering multi-target x layer and MoN layer to form (CrNbTiAlV)CN x / MoN periodic multilayer composite top layer.

[0011] The material of the substrate in step (1) is 8Cr4Mo4V high temperature alloy steel.

[0012] The deposition parameters of the Cr bonding layer in step (3) are: Cr target current is 4.5 A, Ar flow rate is 18 sccm, bias voltage is 60-120 V, substrate rotation speed is 5 rpm, and deposition time is 14 min.

[0013] In the step (3), (CrNbTiAlV)CN x The deposition parameters of the layer are: the current of the multi-component splicing target (Cr-Nb-Ti-Al-V) is 4.5 A, the current of the C target is 4 A, the Ar flow rate is 18 sccm, and the N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 2~20 min.

[0014] The deposition parameters of the MoN layer in step (3) are as follows: Mo target current is 4 A, Ar flow rate is 18 sccm, N 2 The flow rate is 38 sccm, the bias voltage is 50~126 V, the substrate rotation speed is 5 rpm, and the single layer deposition time is 2~20 min.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] 1. The periodic multilayer structure coating of the present invention adopts magnetron sputtering technology to prepare (CrNbTiAlV)CN with different modulation periods by changing the deposition time of the single layer coating. x / MoN multilayer structure coating.

[0017] 2. (CrNbTiAlV)CN prepared by the present invention x The (CrNbTiAlV)CN multilayer composite coating has a smooth interface between layers, a clear and dense periodic structure, and good self-lubricating properties at high temperatures. xThe friction coefficient of the MoN / MoN multilayers at 500 °C is 0.11~0.34, and the bonding force between the coating and the substrate is 65~85 N.

[0018] 3. The present invention adopts magnetron sputtering technology to prepare at room temperature, and the substrate does not need any additional heating process. The N 2 The flow rate and substrate speed remain unchanged. By adjusting the current and deposition time of the multi-component spliced ​​target (Cr-Nb-Ti-Al-V) and Mo target, the modulation period in the multilayer coating is controlled, thereby preparing the (CrNbTiAlV)N with the lowest friction coefficient under a certain modulation period. x / MoN multilayer coating.

[0019] 4. The present invention adopts magnetron sputtering technology, and its preparation process is simple and controllable. Through the periodic multilayer structure design, a functional composite coating with the lowest friction coefficient in a high temperature environment is obtained, which can be used for friction-reducing and wear-resistant parts in a high temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The specific implementation modes of the present invention will be further described in detail below in conjunction with the accompanying drawings.

[0021] Figure 1 (CrNbTiAlV)CN prepared by the present invention x Cross-sectional SEM image of / MoN multilayer coating.

[0022] Figure 2 (CrNbTiAlV)CN prepared by the present invention x / MoN multilayer coating bonding strength.

[0023] Figure 3 (CrNbTiAlV)CN prepared by the present invention x Friction coefficient of / MoN multilayer coatings. DETAILED DESCRIPTION

[0024] A high-temperature self-lubricating periodic multilayer structure coating, the periodic multilayer structure coating comprises a substrate, a Cr bonding layer and a (CrNbTiAlV)CN bonded layer sequentially deposited on the outer surface of the substrate x / MoN top layer composition; the (CrNbTiAlV)CN x / MoN top layer is composed of (CrNbTiAlV)CN x The modulation period is 50~420 nm and the modulation ratio is 1:1~1.2:1.

[0025] The preparation method thereof comprises the following steps:

[0026] ⑴Pre-treat the substrate. The material of the substrate is 8Cr4Mo4V high temperature alloy steel.

[0027] (2) Place the pretreated substrate into a vacuum chamber for evacuation. When the vacuum degree is lower than 1×10 -3 When the substrate surface is 200 Å / s and the ion density is 0.0447 W / m, the substrate surface is sputtered and cleaned by ions to obtain a cleaned substrate.

[0028] ⑶ Using magnetron sputtering technology, a Cr bonding layer is first deposited on the surface of the cleaned substrate, and then (CrNbTiAlV)CN is alternately deposited by magnetron sputtering multi-target x layer and MoN layer to form (CrNbTiAlV)CN x / MoN periodic multilayer composite top layer.

[0029] Among them, the deposition parameters of the Cr bonding layer are: Cr target current is 4.5 A, Ar flow rate is 18 sccm, bias voltage is 60~120 V, substrate rotation speed is 5 rpm, and deposition time is 14 min.

[0030] (CrNbTiAlV)CN x The deposition parameters of the layer are: the current of the multi-component splicing target (Cr-Nb-Ti-Al-V) is 4.5 A, the current of the C target is 4 A, the Ar flow rate is 18 sccm, and the N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 2~20 min.

[0031] The deposition parameters of the MoN layer are as follows: Mo target current 4 A, Ar flow rate 18 sccm, N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 2~20 min.

[0032] Example 1 A method for preparing a high-temperature self-lubricating periodic multilayer structure coating comprises the following steps:

[0033] ⑴ The matrix 8Cr4Mo4V high temperature alloy steel was ultrasonically cleaned with anhydrous ethanol and acetone respectively and then blown dry.

[0034] (2) Place the pretreated substrate into a vacuum chamber for evacuation. When the vacuum degree is lower than 1×10 -3 Pa, Ar was introduced, and the pressure inside the vacuum chamber was maintained at 0.24 Pa. The substrate sample was ion etched with Ar plasma for 25 min to remove the oxide layer and other impurities on the surface to obtain a cleaned substrate.

[0035] ⑶ Using magnetron sputtering technology, a 200 nm thick Cr bonding layer is first deposited on the surface of the cleaned substrate, and then a 230 nm thick (CrNbTiAlV)CN is alternately deposited by magnetron sputtering multi-target. x layer and a MoN layer with a thickness of 190 nm to form (CrNbTiAlV)CN x / MoN periodic multilayer composite top layer.

[0036] Among them, the deposition parameters of the Cr bonding layer are: Cr target current is 4.5 A, Ar flow rate is 18 sccm, bias voltage is 60~120 V, substrate rotation speed is 5 rpm, and deposition time is 14 min.

[0037] (CrNbTiAlV)CN x The deposition parameters of the layer are: the current of the multi-component splicing target (Cr-Nb-Ti-Al-V) is 4.5 A, the current of the C target is 4 A, the Ar flow rate is 18 sccm, and the N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 20 min.

[0038] The deposition parameters of the MoN layer are as follows: Mo target current 4 A, Ar flow rate 18 sccm, N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 20 min.

[0039] Prepared (CrNbTiAlV)CN x The cross-sectional SEM images of the / MoN multilayer composite coating are shown in Figure 2. Figure 1 As shown in (a), the thickness of each period of the coating is 420 nm.

[0040] Example 2 A method for preparing a high-temperature self-lubricating periodic multilayer structure coating comprises the following steps:

[0041] ⑴ The matrix 8Cr4Mo4V high temperature alloy steel was ultrasonically cleaned with anhydrous ethanol and acetone respectively and then blown dry.

[0042] (2) Place the pretreated substrate into a vacuum chamber for evacuation. When the vacuum degree is lower than 1×10 -3 Pa, Ar was introduced, and the pressure inside the vacuum chamber was maintained at 0.24 Pa. The substrate sample was ion etched with Ar plasma for 25 min to remove the oxide layer and other impurities on the surface to obtain a cleaned substrate.

[0043] ⑶ Using magnetron sputtering technology, a 200 nm thick Cr bonding layer is first deposited on the surface of the cleaned substrate, and then a 100 nm thick (CrNbTiAlV)CN is alternately deposited by magnetron sputtering multi-target. x layer and a MoN layer with a thickness of 90 nm to form (CrNbTiAlV)CN x / MoN periodic multilayer composite top layer.

[0044] Among them, the deposition parameters of the Cr bonding layer are: Cr target current is 4.5 A, Ar flow rate is 18 sccm, bias voltage is 60~120 V, substrate rotation speed is 5 rpm, and deposition time is 14 min.

[0045] (CrNbTiAlV)CN x The deposition parameters of the layer are: the current of the multi-component splicing target (Cr-Nb-Ti-Al-V) is 4.5 A, the current of the C target is 4 A, the Ar flow rate is 18 sccm, and the N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 10 min.

[0046] The deposition parameters of the MoN layer are as follows: Mo target current 4 A, Ar flow rate 18 sccm, N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 10 min.

[0047] Prepared (CrNbTiAlV)CN x The cross-sectional SEM images of the / MoN multilayer composite coating are shown in Figure 2. Figure 1 As shown in (b), the thickness of each period of the coating is 190 nm.

[0048] Example 3 A method for preparing a high-temperature self-lubricating periodic multilayer structure coating comprises the following steps:

[0049] ⑴ The matrix 8Cr4Mo4V high temperature alloy steel was ultrasonically cleaned with anhydrous ethanol and acetone respectively and then blown dry.

[0050] (2) Place the pretreated substrate into a vacuum chamber for evacuation. When the vacuum degree is lower than 1×10 -3 Pa, Ar was introduced, and the pressure inside the vacuum chamber was maintained at 0.24 Pa. The substrate sample was ion etched with Ar plasma for 25 min to remove the oxide layer and other impurities on the surface to obtain a cleaned substrate.

[0051] ⑶ Using magnetron sputtering technology, a 200 nm thick Cr bonding layer is first deposited on the surface of the cleaned substrate, and then a 60 nm thick (CrNbTiAlV)CN is alternately deposited by magnetron sputtering multi-target. x layer and a MoN layer with a thickness of 50 nm to form (CrNbTiAlV)CN x / MoN periodic multilayer composite top layer.

[0052] Among them, the deposition parameters of the Cr bonding layer are: Cr target current is 4.5 A, Ar flow rate is 18 sccm, bias voltage is 60~120 V, substrate rotation speed is 5 rpm, and deposition time is 14 min.

[0053] (CrNbTiAlV)CN x The deposition parameters of the layer are: the current of the multi-component splicing target (Cr-Nb-Ti-Al-V) is 4.5 A, the current of the C target is 4 A, the Ar flow rate is 18 sccm, and the N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 5 min.

[0054] The deposition parameters of the MoN layer are as follows: Mo target current 4 A, Ar flow rate 18 sccm, N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 5 min.

[0055] Prepared (CrNbTiAlV)CN x The cross-sectional SEM images of the / MoN multilayer composite coating are shown in Figure 2. Figure 1 As shown in (c), the thickness of each period of the coating is 110 nm.

[0056] Example 4 A method for preparing a high-temperature self-lubricating periodic multilayer structure coating comprises the following steps:

[0057] ⑴ The matrix 8Cr4Mo4V high temperature alloy steel was ultrasonically cleaned with anhydrous ethanol and acetone respectively and then blown dry.

[0058] (2) Place the pretreated substrate into a vacuum chamber for evacuation. When the vacuum degree is lower than 1×10 -3 Pa, Ar was introduced, and the pressure inside the vacuum chamber was maintained at 0.24 Pa. The substrate sample was ion etched with Ar plasma for 25 min to remove the oxide layer and other impurities on the surface to obtain a cleaned substrate.

[0059] ⑶ Using magnetron sputtering technology, a 200 nm thick Cr bonding layer is first deposited on the surface of the cleaned substrate, and then a 25 nm thick (CrNbTiAlV)CN is alternately deposited by magnetron sputtering multi-target. x layer and a MoN layer with a thickness of 25 nm to form (CrNbTiAlV)CN x / MoN periodic multilayer composite top layer.

[0060] Among them, the deposition parameters of the Cr bonding layer are: Cr target current is 4.5 A, Ar flow rate is 18 sccm, bias voltage is 60~120 V, substrate rotation speed is 5 rpm, and deposition time is 14 min.

[0061] (CrNbTiAlV)CN x The deposition parameters of the layer are: the current of the multi-component splicing target (Cr-Nb-Ti-Al-V) is 4.5 A, the current of the C target is 4 A, the Ar flow rate is 18 sccm, and the N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 2 min.

[0062] The deposition parameters of the MoN layer are as follows: Mo target current 4 A, Ar flow rate 18 sccm, N 2 The flow rate was 38 sccm, the bias voltage was 50~126 V, the substrate rotation speed was 5 rpm, and the single layer deposition time was 2 min.

[0063] Prepared (CrNbTiAlV)CN x The cross-sectional SEM images of the / MoN multilayer composite coating are shown in Figure 2. Figure 1 As shown in (d), the thickness of each period of the coating is 50 nm.

[0064] The film-substrate bonding strength of the coatings of Examples 1 to 4 of the present invention was tested using an MFT-4000 scratch tester. The scratch data are as follows: Figure 2 As shown in the figure, it can be seen that with the decrease of the single layer deposition time, the bonding force between the coating and the substrate first decreases and then increases, and the bonding force between the coating and the substrate is 65~85N.

[0065] The tribological properties of the coatings of Examples 1 to 4 of the present invention were tested using a MS-HT1000 high temperature friction tester. The friction balls used were Si with a diameter of 6 mm. 3 N 4 The ball temperature is 500 °C, the normal load is 20 N, the rotation speed is 300 r / min, and the linear speed is 6.28 cm / s. The high temperature friction coefficient results are shown in the attached Figure 3As shown in the figure, (CrNbTiAlV)CN with different modulation periods x The friction coefficient of the MoN / CrNbTiAlV / MoN multilayer coating at 500 °C is 0.11~0.34, among which the (CrNbTiAlV)CN with a modulation period of 110 nm is prepared. x The friction coefficient of the MoN / MoN multilayer coating is the lowest at 500°C, which is about 0.11.

Claims

1. A high-temperature self-lubricating periodic multilayer structure coating, characterized in that: The periodic multilayer structure coating consists of a substrate, a Cr bonding layer and a (CrNbTiAlV)CN layer sequentially deposited on the outer surface of the substrate. x / MoN top layer composition; the (CrNbTiAlV)CN x / MoN top layer is composed of (CrNbTiAlV)CN x The (CrNbTiAlV)CN is obtained by alternately depositing layers and MoN layers, with a modulation period of 50-420nm and a modulation ratio of 1:1-1.2:1; x The deposition parameters of the layer are: the current of the multi-layer spliced ​​target (Cr-Nb-Ti-Al-V) is 4.5 A, the current of the C target is 4 A, the Ar flow rate is 18 sccm, the N2 flow rate is 38 sccm, the bias voltage is 50~126 V, the substrate rotation speed is 5 rpm, and the single layer deposition time is 2~20 min.

2. The method for preparing a high-temperature self-lubricating periodic multilayer structure coating according to claim 1, comprising the following steps: ⑴Pretreat the substrate; (2) Place the pretreated substrate into a vacuum chamber for evacuation. When the vacuum degree is lower than 1×10 -3 When Pa, the substrate surface is sputter-cleaned by bombarding the substrate with ions to obtain a cleaned substrate; ⑶ Using magnetron sputtering technology, a Cr bonding layer is first deposited on the surface of the cleaned substrate, and then (CrNbTiAlV)CN is alternately deposited by magnetron sputtering multi-target x layer and MoN layer to form (CrNbTiAlV)CN x / MoN periodic multilayer composite top layer.

3. The method for preparing a high-temperature self-lubricating periodic multilayer structure coating according to claim 2, characterized in that: The material of the substrate in step (1) is 8Cr4Mo4V high temperature alloy steel.

4. The method for preparing a high-temperature self-lubricating periodic multilayer structure coating according to claim 2, characterized in that: The deposition parameters of the Cr bonding layer in step (3) are: Cr target current is 4.5 A, Ar flow rate is 18 sccm, bias voltage is 60-120 V, substrate rotation speed is 5 rpm, and deposition time is 14 min.

5. The method for preparing a high-temperature self-lubricating periodic multilayer structure coating according to claim 2, characterized in that: The deposition parameters of the MoN layer in step (3) are: Mo target current of 4 A, Ar flow rate of 18 sccm, N2 flow rate of 38 sccm, bias voltage of 50-126 V, substrate rotation speed of 5 rpm, and single layer deposition time of 2-20 min.

Citation Information

Patent Citations

  • CN-MCN superhard self-lubricating nano-composite coating and preparation method thereof

    CN102864411A

  • High-hardness and high-corrosion-resistance high-entropy alloy nitride coating and preparation method thereof