A medium-entropy alloy / metallic glass nanolayered film doped with oxygen and a preparation method thereof
Through the oxygen-doped medium-entropy alloy/metal glass nanolayer film, the alternating laminate structure of oxygen-containing medium-entropy alloy and metal glass layer and the solid solution effect of oxygen atoms are solved, and the brittleness problem of metal glass materials at room temperature is achieved. High strength and uniform plastic deformation have expanded its engineering application prospects.
Patent Information
- Application Number
- CN202410667932.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-05-28
AI Technical Summary
The prior art is difficult to increase the plastic deformation capability of metal glass while maintaining high strength and hardness, resulting in metal glass materials showing brittleness at room temperature, limiting their engineering applications.
Using oxygen-doped medium-entropy alloy/metal glass nano-layer film, the oxygen-containing medium-entropy alloy layer and the oxygen-containing metal glass layer are alternately laminated. By controlling the layer thickness and layer thickness ratio, the solid solution effect and interface of oxygen atoms are combined. The effect is to achieve high strength and uniform plastic deformation of nanolayer films.
It has achieved high strength and large plastic deformation capabilities of nanolayer films, overcomes the brittleness problem of metal glass, and has excellent mechanical properties. It is suitable for high-strength electronic devices, wear-resistant and corrosion-resistant coatings and other fields.
Smart Images

Figure CN118441245B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal alloy films, and in particular relates to an oxygen-doped medium-entropy alloy / metallic glass nano-layered film and a preparation method thereof. Background Art
[0002] Medium / high entropy alloys are new alloys composed of three or more main elements with an atomic ratio of 5% to 35% proposed in the past two decades. Due to the high mixing entropy, this type of alloy easily forms simple face-centered cubic (FCC), body-centered cubic (BCC) and hexagonal close-packed (HCP) crystal structure solid solutions. Their high plasticity usually comes from dislocation slip, twinning or crystal phase transformation. In addition, by controlling the composition and microstructure, the strength of medium / high entropy alloys can be significantly improved, and in some cases even exceeds the strength of traditional crystal alloys. The lattice distortion effect and atomic diffusion of medium / high entropy alloys make it easy for the alloys to form amorphous and precipitate nanocrystalline structures. The cocktail effect makes medium / high entropy alloys have many excellent properties such as high plasticity, high strength, wear resistance and oxidation resistance. They have been widely studied in many fields and can adapt to various environmental requirements. They have very important practical research value.
[0003] Metallic glass, also known as amorphous alloy, was proposed in the 1960s. The atomic structure of this type of material has the characteristics of long-range disorder and short-range order, so it does not have defects such as slip systems and lattice dislocations in crystals, so it exhibits ultra-high yield strength, hardness and good wear resistance. However, the plastic deformation of metallic glass at room temperature mainly depends on the generation and expansion of shear bands, which causes catastrophic damage to metallic glass without any significant macroscopic plasticity. Therefore, metallic glass often exhibits brittleness at room temperature, and its plastic elongation is almost zero, which greatly limits the engineering application of metallic glass. If the plastic deformation capacity of metallic glass can be increased while maintaining its high strength and hardness, then metallic glass materials will have great application prospects.
[0004] As a type of multilayer film material, crystal / amorphous nano-layered composite materials are usually formed by alternating deposition of two or more metals or alloys, and finally form a thin film material with obvious interface and periodic composition changes. It combines the advantages of hard phase amorphous and soft phase crystal, and has high strength and high plasticity. Among them, the crystal / amorphous interface, as a special structure, plays an important role in improving strength, plasticity and strain hardening ability. The amorphous layer can prevent and destroy the movement of dislocations, and the nanocrystalline layer can also inhibit the propagation of shear bands in the amorphous layer, improving the ductility of the material. Therefore, the crystal / amorphous interface is both a high-capacity source of dislocations and a sink of dislocations. At present, in order to inhibit the generation and propagation of shear bands in the amorphous layer, people usually control the thickness of the amorphous layer to less than 20nm, which is the minimum size that shear bands can be generated. However, it is difficult to observe uniform plastic deformation of the amorphous layer at a larger size.
[0005] Therefore, how to prepare high-strength and high-plasticity crystalline / amorphous nano-layered composite materials with larger amorphous layers is a scientific and technological problem that needs to be solved urgently. Summary of the invention
[0006] In order to solve the above technical problems, the present invention proposes an oxygen-doped medium-entropy alloy / metallic glass nano-layered film and a preparation method thereof, so that the prepared nano-layered film has both high strength and high plasticity.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] One of the technical solutions of the present invention:
[0009] An oxygen-doped medium-entropy alloy / metallic glass nano-layered film, comprising an oxygen-containing medium-entropy alloy layer and an oxygen-containing metallic glass layer;
[0010] Among them, the oxygen-containing medium-entropy alloy layer and the oxygen-containing metallic glass layer are stacked in sequence as an alternating period.
[0011] Beneficial effects: The present invention defines that the oxygen-containing medium entropy alloy layer and the oxygen-containing metallic glass layer are stacked as an alternating cycle, wherein the high strength of the amorphous phase, the large number of nano-grain boundaries, stacking faults and high-density crystal / amorphous interfaces of the crystal phase jointly maintain the high strength of the material as a whole; the suitable size and excellent ductility of the crystal phase inhibit the generation and expansion of the shear band of the amorphous phase, which is the key to the uniform plastic deformation ability of the nano-layered film. The nano-crystalline phase, the amorphous phase and the crystal / amorphous heterostructure interface coordinate and interact with each other, so that the nano-layered film has excellent comprehensive mechanical properties.
[0012] In addition, oxygen exists in the film in the form of solid solution. On the one hand, it can occupy the vacancies between metal atoms and produce certain distortions in the lattice points of metal atoms, so that when the crystal layer is subjected to load, it needs greater stress to activate the slip band, which can have a certain strengthening effect on the film. On the other hand, oxygen atoms can act as a barrier to dislocation slip, hindering the movement of dislocations and increasing the strength of the material. Moreover, during deformation, oxygen atoms at the nanograin boundary and the crystal / amorphous interface diffuse between the interfaces, relieving stress concentration, stabilizing the interface, and making a certain contribution to the plasticity of the material.
[0013] Preferably, the oxygen-containing medium-entropy alloy layer is FeCrNiO; and the oxygen-containing metallic glass layer is TiVNbHfO.
[0014] Furthermore, the oxygen-containing medium entropy alloy layer contains Fe 30.5 Cr 26.8 Ni 34.7 O 8.0 ; The oxygen-containing metallic glass layer contains Ti 30.4 V 15.6 Nb 24.1 Hf 14.2 O 15.7 .
[0015] Preferably, the number of alternating cycles is greater than ten.
[0016] Preferably, the thickness of each layer of the oxygen-containing medium entropy alloy layer is 25-100 nm;
[0017] The thickness of each oxygen-containing metallic glass layer is 50 nm, which is larger than the characteristic width of the shear band by 20 nm.
[0018] Beneficial effect: By controlling the thickness of the metallic glass layer and regulating the thickness of the medium-entropy alloy layer, the strength-plasticity trade-off between crystalline materials and amorphous materials can be overcome, giving them excellent mechanical properties.
[0019] The second technical solution of the present invention:
[0020] The method for preparing the above oxygen-doped medium-entropy alloy / metallic glass nano-layered film comprises the following steps:
[0021] By using an alternating sputtering deposition method, an oxygen-containing medium-entropy alloy target material and an oxygen-containing metallic glass target material are alternately sputtered and deposited to obtain the oxygen-doped medium-entropy alloy / metallic glass nano-layered film.
[0022] Beneficial effects: The present invention adopts a DC magnetron sputtering method to alternately deposit a soft phase medium entropy alloy layer and a hard phase metallic glass layer on the substrate surface. The two phases are distributed in alternating layers. The sputtering power and sputtering time of the two phases are regulated to obtain a nano-layered film. By regulating the layer thickness and layer thickness ratio, the nano-layered film has both high strength and excellent plastic deformation ability. Among them, the inherent high yield strength of the metallic glass phase and a large number of crystal / amorphous interfaces contribute to the high strength of the film; the crystal phase inhibits the generation and expansion of the amorphous phase shear band due to its excellent ductility, maintaining the uniform plastic deformation of the entire film.
[0023] Preferably, the sputtering power in the alternating sputtering deposition process is 60 W; the deposition rate is 14-20 nm / min; and the alternating sputtering interval is 30 s.
[0024] Beneficial effects: The film prepared within the alternating sputtering deposition parameters specified in the present invention has good density, close bonding between layers, and excellent mechanical properties; if it is not within this range, the prepared film layers have poor adhesion and weak bonding, and there is even a risk of falling off from the substrate.
[0025] Compared with the prior art, the present invention has the following advantages and technical effects:
[0026] (1) The present invention adopts an alternating sputtering deposition method to adjust the coating parameters, thereby achieving precise control of the thickness of the single layer;
[0027] (2) The nano-layered film prepared by the present invention has a stable and reliable structure, a smooth and straight interface, uniform thickness of each layer, close bonding between the film and the substrate, uniform distribution of internal elements and is dense and non-porous;
[0028] (3) The nano-layered film prepared by the present invention contains a large amount of oxygen atoms in the solid solution, which plays a certain role in solid solution strengthening, making the film tougher and overcoming the prejudice in the prior art that too much oxygen will cause embrittlement;
[0029] (4) The nano-layered film prepared by the present invention has a high yield strength (4.37 GPa) and still exhibits a uniform plastic deformation capacity of 50% (the mechanical property curve is smooth and no shear band appears), has excellent mechanical properties, and has broad application prospects in the fields of high-strength electronic devices, wear-resistant and corrosion-resistant coatings;
[0030] (5) The preparation method defined in the present invention is not limited to the FeCrNi / TiVNbHf alloy system, but can be generally applied to medium (high) entropy alloy / metallic glass, or even medium (high) entropy alloy / medium (high) entropy alloy, metallic glass / metallic glass alloy system, that is, it can realize the combination of single-phase high entropy alloys of different systems;
[0031] (6) The present invention is simple to operate, the conditions are easy to control, the repeatability is good, the process is clean and pollution-free, and it is suitable for large-scale industrialization;
[0032] (7) The amorphous layer thickness in the film prepared by the present invention is larger and is not limited to the shear band thickness (20 nm), but still exhibits high strength and large uniform plastic deformation. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0034] Figure 1 This is a cross-sectional SEM image of the medium-entropy alloy / metallic glass nano multilayer film prepared in Example 2 of the present invention;
[0035] Among them, (b) is the enlarged view of the dotted box in (a);
[0036] Figure 2 The cross-sectional SEM images of the single-component films prepared in Comparative Examples 1 and 2 of the present invention are shown;
[0037] in, Figure 2 (a) is the single-component metallic glass film prepared in Comparative Example 1; (b) is the single-component medium-entropy alloy film prepared in Comparative Example 2;
[0038] Figure 3 This is a cross-sectional HAADF-STEM image of the medium-entropy alloy / metallic glass nano-multilayer film prepared in Example 2 of the present invention;
[0039] Among them, (b) is the EDS line scan image of the composition distribution of the area indicated by the white arrow in (a);
[0040] Figure 4 XRD patterns of the nano multilayer films and single component films prepared in Examples 1-3 and Comparative Examples 1-2 of the present invention;
[0041] Figure 5 The micro-pillar compression engineering stress-strain curves and yield strength comparison diagrams of the nano multi-layer films and single-component films prepared in Examples 1-3 and Comparative Examples 1-2 of the present invention;
[0042] in, Figure 5 (a) is the microcolumn compression engineering stress-strain curve; (b) is the yield strength comparison diagram. DETAILED DESCRIPTION
[0043] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0044] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0045] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0046] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0047] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0048] On the one hand, the present invention provides an oxygen-doped medium-entropy alloy / metallic glass nanolayered film, which is formed by alternating sputtering deposition of medium-entropy alloy layers and metallic glass layers, with the metallic glass layers and the medium-entropy alloy layers as an alternating cycle, the bottom layer being the metallic glass layer, and the top layer being the medium-entropy alloy layer.
[0049] In some preferred embodiments, in the nano-layered film, the metallic glass hard phase layer is TiVNbHfO, and the medium entropy alloy soft phase layer is FeCrNiO.
[0050] In some preferred embodiments, in the nano-layered film, the thickness of the metallic glass layer is controlled to be 50 nm, the thickness of the medium-entropy alloy layer is 25-100 nm, the total number of film layers is greater than 20, and the total thickness of the film is 1.4-1.8 μm.
[0051] On the other hand, the present invention provides a method for preparing an oxygen-doped medium-entropy alloy / metallic glass nano-layered film, comprising the following steps:
[0052] (1) A 0.7 mm thick Si substrate was ultrasonically cleaned with anhydrous ethanol and deionized water in sequence, dried, and placed on a substrate table of an ultra-high vacuum magnetron sputtering device to prepare for coating;
[0053] (2) Using the DC magnetron sputtering method, the metal target is placed on the target table in the chamber, and then the chamber pressure is pumped to high vacuum using a mechanical pump and a molecular pump in turn, with the background vacuum not exceeding 8.0×10 -4 Under the condition of 3.0 Pa, argon gas is introduced, and the gas pressure and gas flow are adjusted. When the vacuum degree of the chamber is 3.0 Pa, the ignition is started, and two metal targets are pre-sputtered on the empty substrate for 10-20 minutes each;
[0054] (3) After pre-sputtering, the vacuum degree of the chamber is adjusted to 0.3 Pa for formal coating. The metallic glass hard phase layer is first coated, and then the medium-entropy alloy soft phase layer is coated. The power is controlled to 60 W, and the deposition rates of the hard phase layer and the soft phase layer are 14-20 nm / min. The thickness of the hard phase layer and the soft phase layer is controlled by controlling the sputtering deposition time to ensure that the layer thickness reaches the set expectation. The hard phase layer is coated first and then the soft phase layer is coated alternately to obtain an oxygen-doped medium-entropy alloy / metallic glass nanolayered film.
[0055] In some preferred embodiments, in step (1), the Si substrate is a single crystal Si with a (100) crystal plane orientation; in step (1), the single crystal Si substrate is ultrasonically cleaned with anhydrous ethanol and deionized water in sequence for 10-20 minutes.
[0056] In some preferred embodiments, in step (2), the metal alloy target is Ti 30.4 V 15.6 Nb 24.1 Hf 14.2 O 15.7 (at.%) and Fe 30.5 Cr 26.8 Ni 34.7 O 8.0 (at.%).
[0057] In some preferred embodiments, in step (2), the inlet flow rate of argon gas is 40.0 sccm.
[0058] In some preferred embodiments, in step (3), after a layer of thin film is sputtered, wait for 30 seconds before sputtering and depositing another layer of thin film.
[0059] In some preferred embodiments, in step (3), under the condition of a power of 60 W for both metal alloy targets, the deposition rate of the TiVNbHfO layer is 18 nm / min, and the deposition rate of the FeCrNiO layer is 14 nm / min.
[0060] All raw materials used in the embodiments of the present invention are purchased from the market. Among them, the magnetron sputtering deposition system used in the embodiments of the present invention is a high-throughput magnetron sputtering deposition system model JGP-560 produced by Shenyang Scientific Instrument Co., Ltd., Chinese Academy of Sciences; Ti 30.4 V 15.6 Nb 24.1 Hf 14.2 O 15.7 (at.%) and Fe 30.5 Cr 26.8 Ni 34.7 O 8.0 (at.%) alloy target was purchased from Nanjing Mingchang New Material Technology Co., Ltd., with a target diameter of 50 mm and a thickness of 4 mm.
[0061] Unless otherwise specified, the “parts” used in the embodiments of the present invention are “parts by weight”.
[0062] The technical solution of the present invention is further illustrated by the following embodiments.
[0063] Example 1
[0064] (1) The surfaces of the TiVNbHfO and FeCrNiO targets were cleaned with an electric brush to remove the surface oxide film, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 min respectively. After drying, they were fixed on two DC power supply target stages of the magnetron sputtering system respectively; the (100) Si substrate was ultrasonically cleaned with anhydrous ethanol and deionized water for 10 min respectively, and after drying, it was adhered to the sample substrate with high-temperature tape.
[0065] (2) After the preparation work is completed, close the chamber, start the system, and use the mechanical pump and molecular pump to pump the chamber pressure to high vacuum. When the vacuum pressure reaches 8×10 -4 When argon gas is introduced, the gas flow rate is controlled to be 40 sccm, and the cavity pressure is maintained at 3 Pa by controlling the molecular pump valve.
[0066] (3) Turn on the DC power supply of the TiVNbHfO target, adjust the power to 60W for glowing, wait for the glow to stabilize, and pre-sputter for 20 minutes on the sample stage without substrate to clean the impurities and oxides on the surface of the target. After pre-sputtering the TiVNbHfO target, turn on the DC power supply of the FeCrNiO target and pre-sputter the FeCrNiO target for 20 minutes.
[0067] (4) After pre-sputtering, the vacuum of the chamber was adjusted to 0.3 Pa, the argon flow rate was 40 sccm, and the coating was carried out. The TiVNbHfO layer was first coated with a power of 60 W and a deposition rate of 18 nm / min. After the TiVNbHfO layer was coated, it was stopped for 30 seconds, and then the FeCrNiO layer was coated with a power of 60 W and a deposition rate of 14 nm / min. The deposition time was controlled to make the thickness of each TiVNbHfO layer 50 nm and the thickness of each FeCrNiO layer 25 nm. Two layers were one cycle, and then 22 cycles were alternately deposited to obtain FeCrNiO / TiVNbHfO C25 / A50 nanolayered film.
[0068] Finally, the actual measured compositions of the two layers of the nano-layered film prepared in this embodiment are Ti 30.4 V 15.6 Nb 24.1 Hf 14.2 O 15.7 (at.%) and Fe 30.5 Cr 26.8 Ni 34.7 O 8.0 (at.%) (which is the same as that of the target material in the raw material, and the same is true for Example 3), and the actual measured film thickness is 1.68μm. Figure 4 The XRD pattern shown shows obvious amorphous peaks and broad (111) crystalline peaks. Figure 5 The micropillar compressive yield strength shown is 4.44 ± 0.07 GPa.
[0069] Example 2
[0070] The difference from Example 1 is that
[0071] (4) By controlling the deposition time, the thickness of the TiVNbHfO layer is about 50 nm, and the thickness of the FeCrNiO layer is about 50 nm. Two layers constitute one cycle, and then 16 cycles are alternately deposited to obtain a FeCrNiO / TiVNbHfO C50 / A50 nanolayered film.
[0072] Finally, the actual measured compositions of the two layers of the nano-layered film prepared in this embodiment are Fe 30.5 Cr 26.8 Ni 34.7 O 8.0 (at.%),Ti 30.4 V 15.6 Nb 24.1 Hf 14.2 O 15.7(at.%) (the actual content of each element in the prepared film is related to its vapor pressure, segregation, diffusion and other factors; the content in the layered film is also affected by atomic diffusion and segregation at the interface; in addition, due to the relatively limited resolution of SEM and TEM, the element content in the film layer finally measured will be different from that of the alloy target). The thickness of the nano-layered film prepared in this embodiment is measured to be 1.48 μm. Figure 1 As shown, there are clear boundaries between layers and the texture is uniform. Figure 4 The XRD pattern shown shows obvious amorphous peaks and broad (111) crystalline peaks. Figure 5 The micropillar compressive yield strength is shown to be 4.37±0.09 GPa.
[0073] Example 3
[0074] The difference from Example 1 is that
[0075] (4) By controlling the deposition time, the thickness of the TiVNbHfO layer is about 50 nm, and the thickness of the FeCrNiO layer is about 100 nm. Two layers constitute one cycle, and then 11 cycles are alternately deposited to obtain the FeCrNiO / TiVNbHfO C100 / A50 nanolayered film.
[0076] The thickness of the nano-layered film obtained in this embodiment was finally measured to be 1.67 μm. Figure 4 The XRD pattern shown shows obvious amorphous peaks and broad (111) crystalline peaks. Figure 5 The micropillar compressive yield strength is shown to be 3.78±0.06GPa.
[0077] Comparative Example 1
[0078] (1) The surface of the TiVNbHfO target was cleaned with an electric brush to remove the surface oxide film, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes respectively. After drying, it was fixed on the target stage of the magnetron sputtering system; the (100)Si substrate was ultrasonically cleaned with anhydrous ethanol and deionized water for 10 minutes respectively, and after drying, it was adhered to the sample substrate with high-temperature tape.
[0079] (2) After the preparation work is completed, close the chamber, start the system, and use the mechanical pump and molecular pump to pump the chamber pressure to high vacuum. When the vacuum pressure reaches 8×10 -4 When argon gas is introduced, the gas flow rate is controlled to be 40 sccm, and the cavity pressure is maintained at 3 Pa by controlling the molecular pump valve.
[0080] (3) Turn on the DC power supply of the TiVNbHfO target and adjust the power to 60 W for glow. After the glow stabilizes, pre-sputter for 20 minutes on the sample stage without a substrate to clean the impurities and oxides on the target surface.
[0081] (4) After pre-sputtering, the vacuum degree of the chamber was adjusted to 0.3 Pa, the argon gas flow rate was 40 sccm, and the coating was carried out. The TiVNbHfO layer was coated with a power of 60 W and a deposition rate of 18 nm / min. The sputtering deposition was stopped after 85 min to obtain a single-component TiVNbHfO metallic glass film.
[0082] Finally, the actual measured composition of the single-component TiVNbHfO metallic glass film prepared in this embodiment is Ti 35.6 V 17.2 Nb 22.3 Hf 17.5 O 7.4 (at.%). The thickness is 1.65 μm, such as Figure 2 (a) shown. Figure 4 The XRD pattern shown shows obvious amorphous peaks. Figure 5 The micropillar compressive yield strength is shown to be 4.97±0.08GPa.
[0083] Comparative Example 2
[0084] (1) The surface of the FeCrNiO target was cleaned with an electric brush to remove the surface oxide film, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes respectively. After drying, it was fixed on the target stage of the magnetron sputtering system; the (100)Si substrate was ultrasonically cleaned with anhydrous ethanol and deionized water for 10 minutes respectively, and after drying, it was adhered to the sample substrate with high-temperature tape.
[0085] (2) After the preparation work is completed, close the chamber, start the system, and use the mechanical pump and molecular pump to pump the chamber pressure to high vacuum. When the vacuum pressure reaches 8×10 -4 When argon gas is introduced, the gas flow rate is controlled to be 40 sccm, and the cavity pressure is maintained at 3 Pa by controlling the molecular pump valve.
[0086] (3) Turn on the DC power supply of the FeCrNiO target and adjust the power to 60 W for glow. After the glow is stable, pre-sputter for 20 minutes on the sample stage without substrate to clean the impurities and oxides on the target surface.
[0087] (4) After pre-sputtering, the vacuum degree of the chamber was adjusted to 0.3 Pa, the argon gas flow rate was 40 sccm, and the FeCrNiO layer was coated with a power of 60 W and a deposition rate of 14 nm / min. The sputtering deposition was stopped after 120 min to obtain a single-component FeCrNiO medium-entropy alloy film.
[0088] The composition of the single-component FeCrNiO entropy alloy film prepared in this embodiment is measured to be Fe 28.0 Cr 29.8 Ni 28.9 O 13.3 (at.%). The thickness is 1.77 μm. Figure 2 (b) as shown. Figure 4 The XRD pattern shown shows a broadened (111) crystal peak. Figure 5 The micropillar compressive yield strength is shown to be 2.98±0.19 GPa.
[0089] Figure 3 This is an EDS line scanning image of the cross-section HAADF-STEM of the medium-entropy alloy / metallic glass nano-multilayer film prepared in Example 2. The nano-layered film prepared in Example 2 has a certain degree of oxygen content, and the oxygen mainly exists in the form of solid solution. The oxygen content of the TiVNbHfO layer is slightly greater than that of the FeCrNiO layer because the average atomic radius of the TiVNbHfO layer is larger and can accommodate more oxygen.
[0090] Figure 4 The XRD patterns of the nano multilayer films and single component films prepared in Examples 1-3 and Comparative Examples 1-2 of the present invention are shown. The single component metallic glass film prepared in Comparative Example 1 has only obvious amorphous diffraction peaks, indicating that the film is a pure amorphous phase. The single component medium entropy alloy film prepared in Comparative Example 2 has a wide (111) crystal texture, indicating that the film is pure nanocrystalline. The nano layered films prepared in Examples 1-3 have both obvious amorphous peaks and wide (111) crystal peaks, indicating that the films are coexistent nanocrystalline and amorphous, and as the crystal layer thickness increases (Examples 1 to 3), the intensity of the amorphous peak gradually decreases, and the crystal (111) peak gradually increases, indicating that the crystal phase content gradually increases and the amorphous phase content gradually decreases.
[0091] Figure 5 The micro-pillar compression engineering stress-strain curves and yield strength comparison diagrams of the nano multilayer films and single-component films prepared in Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG. Figure 5It can be seen that compared with Comparative Example 1, although the yield of the films obtained in Examples 1-3 is reduced, the uniform deformation is greatly increased, which is shown in the figure as a smoother mechanical property curve and a smaller stress mutation. Compared with Comparative Example 2, although the uniform plastic deformation ability of the films obtained in Examples 1-3 is slightly poor, the yield strength is greatly improved. Therefore, the medium-entropy alloy / metallic glass nano-layered film obtained in the embodiment has ultra-high strength while maintaining uniform plastic deformation ability, partly because the presence of oxygen plays a role in solid solution strengthening. More importantly, the increase in strength shows that the metallic glass layer and the crystal / amorphous interface can improve the overall strength of the nano-layered film, and the medium-entropy alloy layer can inhibit the generation and expansion of shear bands in the metallic glass layer, thereby achieving uniform plastic deformation. And from Figure 5 As can be seen in (b), the overall strength of the nanolayered film is also higher than the theoretical value calculated by the mixing rule.
[0092] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. An oxygen-doped medium-entropy alloy / metallic glass nanolayer film, It is characterized in that including an oxygen-containing medium-entropy alloy layer and an oxygen-containing metallic glass layer; Among them, the oxygen-containing medium-entropy alloy layer and the oxygen-containing metallic glass layer are stacked in sequence as an alternating cycle; The oxygen-containing medium entropy alloy layer contains Fe 30.5 Cr 26.8 Ni 34.7 O 8.0 ; The oxygen-containing metallic glass layer contains Ti 30.4 V 15.6 Nb 24.1 Hf 14.2 O 15.7 ; The thickness of each layer of the oxygen-containing medium entropy alloy layer is 25-100 nm; The thickness of each oxygen-containing metallic glass layer is 50 nm.
2. The oxygen-doped medium-entropy alloy / metallic glass nanolayered film according to claim 1, It is characterized in that The number of alternating cycles is greater than ten.
3. The method for preparing the oxygen-doped medium-entropy alloy / metallic glass nano-layered film according to any one of claims 1 to 2, It is characterized in that The following steps are involved: By using an alternating sputtering deposition method, an oxygen-containing medium-entropy alloy target and an oxygen-containing metallic glass target are alternately sputtered and deposited to form an oxygen-containing medium-entropy alloy layer and an oxygen-containing metallic glass layer, thereby obtaining the oxygen-doped medium-entropy alloy / metallic glass nanolayered film.
4. The method for preparing the oxygen-doped medium-entropy alloy / metallic glass nano-layered film according to claim 3, It is characterized in that The sputtering power in the alternating sputtering deposition process was 60 W; the deposition rate was 14-20 nm / min; and the alternating sputtering interval was 30 s.