A paramagnetic micron material and preparation method thereof

Through constant-temperature magnetic stirring and calcination, the cathode material of waste lithium iron phosphate batteries is transformed into paramagnetic micron materials, which solves the environmental pollution problem caused by the recycling method of lithium iron phosphate and achieves low-cost and efficient recycling.

CN115947379BActive Publication Date: 2024-10-22JIANGSU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211723150.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-22
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Existing lithium iron phosphate recovery methods are prone to environmental pollution, mainly due to the need to consume a large amount of chemical reagents and discharge a large amount of salty wastewater during the hydrometallurgical process.

Method used

Using a constant-temperature magnetic stirrer, the positive electrode material of the waste lithium iron phosphate battery is stirred and calcined in an alkali solution to obtain paramagnetic micron materials, which avoids the use of large amounts of chemical reagents and the discharge of salty wastewater.

Benefits of technology

This method is simple to operate and low in cost, achieves effective recycling of lithium iron phosphate, reduces environmental pollution during the recycling process, and improves the added value and utilization rate of waste lithium iron phosphate battery recycling products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947379B_ABST
    Figure CN115947379B_ABST
Patent Text Reader

Abstract

The present invention provides a paramagnetic micron material and a preparation method thereof, which relates to the technical field of power batteries, and comprises the following steps: S1: placing the positive electrode of a waste lithium iron phosphate battery into an alkaline solution, stirring on a constant temperature magnetic stirrer to obtain a mixture; S2: filtering the mixture to obtain a filter residue and a filtrate; S3: drying the filter residue, and calcining at 400°C-600°C to obtain a paramagnetic micron material. The preparation method of the paramagnetic micron material provided by the present invention uses the positive electrode material of the waste lithium iron phosphate battery as a raw material, and directly converts Fe and O in the lithium iron phosphate into micron-grade paramagnetic Fe3O4 through stirring and calcining with a constant temperature magnetic stirrer. The method is simple to operate, has a low preparation cost, does not require the consumption of a large amount of chemical reagents, does not discharge a large amount of saline wastewater, and is not prone to environmental pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of power batteries, and in particular to a paramagnetic micron material and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the characteristics of high energy density, high power, and long life. They have been recognized as new energy storage and conversion devices for electric vehicles, which are beneficial to protecting the environment and solving energy problems. Among various lithium-ion batteries, lithium iron phosphate occupies a large share of the lithium-ion battery market due to its safety, thermal stability, non-toxicity, and long service life. At the same time, a large number of waste lithium iron phosphate batteries will be generated, and environmentally feasible and economically feasible methods are needed to recycle waste batteries to curb waste lithium ion environmental toxic waste and inhibit the depletion of remaining lithium resources. At present, the recycling methods and process routes of waste lithium-ion batteries have been widely developed. The hydrometallurgical method is the most commonly used method for recycling waste lithium iron phosphate, that is, using acid or alkaline solutions to transfer metal ions from electrode materials to leaching solutions, and then selectively separating Li, Fe and P in the form of salt. In the hydrometallurgical process, a large amount of chemical reagents need to be consumed, a large amount of saline wastewater is discharged, and the organic electrolyte cannot be well recycled and treated, which is easy to cause environmental pollution. These shortcomings greatly hinder the effective recycling of waste lithium iron phosphate.

[0003] In view of this, it is imperative to develop a new method for recycling waste lithium iron phosphate batteries. Summary of the invention

[0004] The problem solved by the present invention is that the existing lithium iron phosphate recovery method is prone to cause environmental pollution.

[0005] In order to solve the above problems, the present invention provides a method for preparing a paramagnetic micron material, comprising the following steps:

[0006] S1: placing the positive electrode of the waste lithium iron phosphate battery into an alkaline solution and stirring on a constant temperature magnetic stirrer to obtain a mixture;

[0007] S2: filtering the mixture to obtain a filter residue and a filtrate;

[0008] S3: After drying the filter residue, calcining it at 400° C.-600° C. to obtain a paramagnetic micron material.

[0009] Optionally, the temperature range of the constant temperature magnetic stirring is 15-60°C.

[0010] Optionally, the rotation speed of the constant temperature magnetic stirring is 250 rpm.

[0011] Optionally, the calcination time in step S3 is 1-5h.

[0012] Optionally, the alkali solution is NaOH solution.

[0013] Optionally, the concentration range of the NaOH solution is 0.2 mol / L-1 mol / L.

[0014] Optionally, the method further includes: S4: recovering lithium and aluminum in the filtrate.

[0015] Another object of the present invention is to provide a paramagnetic micron material, which is prepared by the method for preparing the paramagnetic micron material as described above.

[0016] Compared with the prior art, the preparation method of the paramagnetic micron material provided by the present invention has the following advantages:

[0017] The preparation method of the paramagnetic micron material provided by the present invention uses the positive electrode material of waste lithium iron phosphate batteries as raw materials, and directly converts Fe and O in the lithium iron phosphate into micron-grade paramagnetic Fe3O4 through stirring and calcination with a constant temperature magnetic stirrer. The method is simple to operate, has a low preparation cost, does not require the consumption of a large amount of chemical reagents, does not discharge a large amount of salt-containing wastewater, and is not prone to causing environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the XRD pattern of the paramagnetic micron material prepared in Example 1 of the present invention;

[0019] Figure 2 This is a SEM image of the paramagnetic micron material prepared in Example 2 of the present invention;

[0020] Figure 3 This is the hysteresis loop of the paramagnetic micron material prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0021] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but are not to be construed as limiting the present invention. All other embodiments obtained by ordinary technicians in the field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.

[0022] In order to solve the problem that the existing lithium iron phosphate recovery method is prone to cause environmental pollution, the present invention provides a method for preparing a paramagnetic micron material, comprising the following steps:

[0023] S1: placing the positive electrode of the waste lithium iron phosphate battery into an alkaline solution and stirring on a constant temperature magnetic stirrer to obtain a mixture;

[0024] S2: filtering the mixture to obtain a filter residue and a filtrate;

[0025] S3: After drying the filter residue, calcining it at 400°C-600°C to obtain a paramagnetic micron material.

[0026] Specifically, the present invention preferably cuts the LiFePO4 positive electrode scraps into small pieces of 1cm×1cm, stirs them on a constant temperature magnetic stirrer until the current collector aluminum is completely dissolved to obtain a mixture; through the stirring action of the constant temperature magnetic stirrer, while fully stirring so that the lithium iron phosphate is fully dissolved, the iron element is made paramagnetic based on the principle of magnetic stirring; and after further drying and calcining the filter residue in the mixture, a paramagnetic micron material can be obtained.

[0027] The preparation method of the paramagnetic micron material provided by the present invention uses the positive electrode material of waste lithium iron phosphate batteries as raw materials, and directly converts Fe and O in the lithium iron phosphate into micron-grade paramagnetic Fe3O4 through stirring and calcination with a constant temperature magnetic stirrer. The method is simple to operate, has a low preparation cost, does not require the consumption of a large amount of chemical reagents, does not discharge a large amount of salt-containing wastewater, and is not prone to causing environmental pollution.

[0028] Specifically, the preferred constant temperature magnetic stirring temperature range is 15-60° C., and the rotation speed is 250 rpm; the preferred calcination time in step S3 is 1-5 h.

[0029] The alkali solution may be a NaOH solution or a KOH solution. In the present invention, the alkali solution is preferably a NaOH solution, and further preferably, the concentration range of the NaOH solution is 0.2 mol / L-1 mol / L.

[0030] Furthermore, the method for preparing the paramagnetic micron material provided by the present invention further comprises: S4: recovering lithium and aluminum in the filtrate.

[0031] The specific method for recovering lithium and aluminum in the filtrate can be selected from the relevant methods in the prior art; the present application does not limit the specific method for recovering lithium and aluminum.

[0032] Another object of the present invention is to provide a paramagnetic micron material, which is prepared by the method for preparing the paramagnetic micron material as described above.

[0033] The paramagnetic micron material provided by the present invention is prepared with the positive electrode material of waste lithium iron phosphate batteries as raw materials. During the preparation process, Fe and O in the lithium iron phosphate are directly converted into micron-grade paramagnetic Fe3O4 through stirring and calcination with a constant temperature magnetic stirrer. The method is simple to operate, has a low preparation cost, does not require the consumption of a large amount of chemical reagents, does not discharge a large amount of salt-containing wastewater, and is not prone to causing environmental pollution.

[0034] Compared with ordinary Fe3O4, paramagnetic Fe3O4 has broader application prospects in the fields of biomedicine, immunity, environmental science, etc. The preparation method of the paramagnetic micron material provided by the present invention uses the positive electrode material of waste lithium iron phosphate batteries as raw materials to prepare paramagnetic Fe3O4, which not only realizes the effective recycling of waste lithium iron phosphate, reduces the discharge of salt-containing wastewater during the recycling process, but also increases the added value of the recycled products of waste lithium iron phosphate batteries and improves the utilization rate.

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0036] Example 1

[0037] The present invention provides a method for preparing a paramagnetic micron material, comprising the following steps:

[0038] S1: Cut the leftover LiFePO4 positive electrode into small pieces of 1 cm×1 cm, take 1 g and put it into a beaker containing 100 ml of 0.5 mol / L NaOH solution, place the beaker on a constant temperature magnetic stirrer and stir at a stirring temperature of 25°C and a stirring speed of 250 rpm until the current collector aluminum is completely dissolved to obtain a mixture;

[0039] S2: filtering the mixture and washing it with deionized water for several times to obtain a filter residue and a filtrate;

[0040] S3: After drying the filter residue, move it to a tubular furnace and calcine it at 550°C for 2 hours with air. The obtained sample is a micron-sized Fe3O4 sample, i.e. a paramagnetic micron material.

[0041] The prepared paramagnetic micron material was tested, see Figure 1 As shown, compared with the standard spectrum, it is the Fe3O4 sample of JCPDS:019-0629.

[0042] Example 2

[0043] The present invention provides a method for preparing a paramagnetic micron material, comprising the following steps:

[0044] S1: Cut the leftover LiFePO4 cathode into 1 cm × 1 cm pieces, take 2 g and put it into a beaker containing 100 ml of 1 mol / L NaOH solution, place the beaker on a constant temperature magnetic stirrer and stir at a temperature of 35 ° C and a speed of 300 rpm until the current collector aluminum is completely dissolved to obtain a mixture;

[0045] S2: filtering the mixture and washing it with deionized water for several times to obtain a filter residue and a filtrate;

[0046] S3: After drying the filter residue, move it to a tubular furnace and calcine it at 550°C for 4 hours in air. The obtained sample is a micron-sized Fe3O4 sample, i.e. a paramagnetic micron material.

[0047] The prepared paramagnetic micron material was tested, see Figure 2 As shown, the paramagnetic micron material prepared in this embodiment is in the form of irregular powder with a size of micron level.

[0048] Example 3

[0049] The present invention provides a method for preparing a paramagnetic micron material, comprising the following steps:

[0050] S1: Cut the leftover LiFePO4 positive electrode into small pieces of 1 cm×1 cm, take 1 g and put it into a beaker containing 100 ml of 0.75 mol / L NaOH solution, place the beaker on a constant temperature magnetic stirrer and stir at a stirring temperature of 25°C and a stirring speed of 300 rpm until the current collector aluminum is completely dissolved to obtain a mixture;

[0051] S2: filtering the mixture and washing it with deionized water for several times to obtain a filter residue and a filtrate;

[0052] S3: After drying the filter residue, move it to a tubular furnace and calcine it at 550°C for 4 hours in air. The obtained sample is a micron-sized Fe3O4 sample, i.e. a paramagnetic micron material.

[0053] The prepared paramagnetic micron material was tested, see Figure 3 As shown, the paramagnetic micron material prepared in this embodiment has a saturation magnetization intensity of 11.19 emu / g, has a certain magnetism, and the hysteresis loops basically overlap, indicating that the material is paramagnetic.

[0054] Comparative Example 1

[0055] This comparative example provides a method for recovering waste lithium iron phosphate, which comprises the following steps:

[0056] S1: Cut the leftover LiFePO4 positive electrode into small pieces of 1 cm×1 cm, take 2 g and put it into a beaker of 100 ml 0.5 mol / L NaOH solution, stir it with a stirrer at a temperature of 40°C and a speed of 250 rpm, and stir the reaction until the current collector aluminum is completely dissolved to obtain a mixture;

[0057] S2: filtering the mixture and washing it with deionized water for several times to obtain a filter residue and a filtrate;

[0058] S3: After drying the filter residue, move it to a tubular furnace and calcine it at 550° C. for 2 h in air to obtain a micron material.

[0059] The paramagnetism of the micron material prepared in this comparative example was tested, and the testing process was the same as that of Example 3; according to the test results, it can be seen that the micron material does not have paramagnetism.

[0060] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing a paramagnetic micron material, characterized in that: The steps include: S1: Cut the LiFePO4 positive electrode scraps of the waste lithium iron phosphate battery into small pieces of 1 cm×1 cm and put them into an alkaline solution, and stir the reaction on a constant temperature magnetic stirrer until the current collector aluminum is completely dissolved to obtain a mixture; the temperature range of the constant temperature magnetic stirring is 15-35° C.; the alkaline solution is a NaOH solution with a concentration range of 0.2 mol / L-1 mol / L; the speed of the constant temperature magnetic stirring is 300 rpm; S2: filtering the mixture to obtain a filter residue and a filtrate; S3: After drying the filter residue, calcining it at 550° C. for 2-5 hours to obtain a paramagnetic micron material.

2. The method for preparing the paramagnetic micron material according to claim 1, characterized in that: Also includes: S4: recovering lithium and aluminum in the filtrate.