Complex and its application in preparation of heavy catalytic cracking catalyst resistant to metal pollution

By contacting the complex formed by modified metal ions and macromolecular complexing agents with the surface of the catalyst precursor microspheres, a metal pollution-resistant catalyst is formed, which solves the problem of high hydrogen to methane ratio and high hydrogen production rate of the catalyst under high nickel pollution conditions. problem, achieving good anti-nickel pollution effect and high-value product distribution at low modified metal content.

CN115957799BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202111190221.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-13
Publication Date
2024-10-11
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

Under conditions of high nickel pollution, it is difficult for existing catalytic cracking catalysts to effectively reduce the hydrogen-to-methane ratio and optimize the distribution of high-value products, and the commonly used antimony-based metal passivators are highly toxic and affect environmental protection requirements.

Method used

The complex formed by modified metal ions and macromolecular complexing agent is used to contact the surface of the catalyst precursor microsphere through spray impregnation or equal volume impregnation method to form complex clusters with larger dynamic diameter, forming Catalyst that resists metal contamination and reduces the dehydrogenation activity of nickel.

Benefits of technology

At low modified metal content, it can significantly improve the catalyst's resistance to nickel pollution, reduce hydrogen and coke yields, optimize the distribution of high-value products, such as increasing LPG and gasoline yields, reducing hydrogen to methane ratio, and has a certain anti-vanadium pollution effect .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115957799B_ABST
    Figure CN115957799B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalytic material preparation, and relates to a complex and its application in the preparation of a heavy catalytic cracking catalyst resistant to metal pollution. The complex comprises a modified metal ion and a complexing agent, the molar ratio of the complexing agent to the modified metal ion is 0.5:1-10:1, the modified metal is one or more of Ti, Mn, Ba, and Ca, and the complexing agent is a macromolecular complexing agent. The complex is used to introduce a modified metal element of an anti-pollution metal into a catalytic cracking catalyst, and a good anti-metal pollution effect can be achieved under the condition of a low content of the modified metal.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The invention relates to a catalytic cracking catalyst used in a fluidized catalytic cracking process, and in particular to the preparation and application of a catalyst for improving the nickel tolerance of heavy oil catalytic cracking to process heavy raw materials. Background of the Invention

[0002] Fluid catalytic cracking (FCC) technology has become an important means of secondary processing of heavy oil in the world today because of its low investment, strong adaptability to raw materials and simple operation, and catalytic cracking catalyst plays a key role in this process. With the increasing depletion of high-quality light crude oil resources worldwide and the increase in delayed coking capacity, refineries have been blending a large proportion of low-quality crude oil such as residual oil, coking wax oil and deasphalted oil in catalytic cracking units in order to increase efficiency, which has a serious impact on the stable operation of catalytic cracking units and the distribution of cracking products, and has put forward higher requirements on the performance of catalytic cracking catalysts.

[0003] Since residual oil feed usually contains pollutant metals such as Ni, V, Fe, Na, and Ca, heavy metals such as nickel and vanadium in the feed oil are continuously deposited on the catalyst surface during the use of catalytic cracking catalysts, causing certain toxic effects on the catalysts. For example, Ni can induce dehydrogenation and significantly increase the yield of H2 and coke; V easily interacts with zeolite under high-temperature hydrothermal conditions to destroy its skeleton structure. Alkaline metals such as sodium and calcium easily destroy the active center of the catalyst. Therefore, the catalyst needs to have a certain passivation component or metal space to prevent metal pollution from affecting the catalyst activity and product distribution.

[0004] Ni has a great influence on the selectivity of the reaction. With the increase of Ni content in the catalyst of the catalytic cracking unit, a strong catalytic dehydrogenation effect is shown, the hydrogen coke yield increases, and high-value products such as gasoline and LPG are affected. In addition, the high hydrogen yield will also put the gas compressor under greater pressure. Studies have shown that nickel and the matrix in the catalyst can form high-priced and difficult-to-reduce nickel aluminate or nickel aluminosilicate, but the formation of stable nickel aluminate or nickel aluminosilicate requires multiple reduction-regeneration cycles, and new nickel is continuously deposited. Therefore, there is always a part of nickel that can be completely or partially reduced. "Active nickel". Various refineries at home and abroad suppress the dehydrogenation toxicity of this part of "active nickel" by adding a passivating Ni agent during the reaction. The passivating Ni agent is often injected into the cracking reactor in an oil-soluble or water-soluble liquid state. During the reaction, its effective components contact the catalyst surface and act on the "active nickel" on the catalyst surface to make it lose its toxicity. Since antimony has the best passivation effect on nickel toxicity, the most commonly used antimony-type metal passivator in China is currently used. Studies have shown that antimony and reduced nickel form stable nickel antimonite NiSb x O y, thereby changing the electronic properties of Ni and thus passivating the Ni dehydrogenation activity.

[0005] Therefore, in the face of increasingly stringent environmental protection requirements, preparing catalysts with high nickel tolerance and being able to passivate the active nickel on the catalyst surface without the use of highly toxic antimony Sb is an important means to reduce hazardous waste from the source.

[0006] One method of preparing metal pollution-resistant catalysts is to use macroporous materials so that the metal is mainly deposited in the macroporous materials. Another method is to add some modified metals. However, existing metal pollution-resistant catalysts still have the problem of poor nickel resistance and high hydrogen and methane in cracking products. Even the inappropriate introduction of some metals will lead to an increased tendency of catalyst coking and an increase in coke yield. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a heavy oil catalytic cracking catalyst with high nickel tolerance, wherein the catalytic cracking catalyst can have a lower hydrogen-methane ratio and optimize the distribution of high-value products under high nickel contamination conditions.

[0008] Another technical problem to be solved by the present invention is to provide a method for preparing the catalyst.

[0009] The third technical problem to be solved by the present invention is to provide a complex for preparing the above catalyst.

[0010] A complex for improving the metal resistance of a catalytic cracking catalyst, comprising a modified metal ion and a complexing agent, wherein the molar ratio of the complexing agent to the modified metal ion is 0.5:1 to 10:1, the modified metal is one or more of Ti, Mn, Ba, and Ca, and the complexing agent is a macromolecular complexing agent. The macromolecular complexing agent in the complex can fully complex with the metal to form a complex and / or complex cluster with a larger kinetic diameter, preferably, the molecular kinetic diameter of the complex and complex cluster is not less than 5 nm, for example, 5 to 100 nm, for example, not less than 10 nm, for example, 10 to 50 nm.

[0011] According to the complex described in the above technical solution, the macromolecular complexing agent is one or more of polypyridine, EDTA, EDTA derivatives, macromolecular organic acids, macromolecular organic acid salts, NTA (aminotriacetic acid), EDDS (ethylenediamine disuccinic acid), PEI (polyetherimide), o-phenanthroline, pyrophosphate, and polyphosphate; preferably one or more of acids such as EDTA, ethylenediaminetetraacetic acid, EDDS (ethylenediamine disuccinic acid), pyrophosphate and polyphosphoric acid and salts of the above acids; the molar ratio of the macromolecular complexing agent molecules to the metal ions is preferably 0.5 to 6:1, preferably 1.0 to 4:1.

[0012] The method for preparing the complex described in any of the above technical solutions comprises the following steps:

[0013] (1) mixing a modified metal compound, a macromolecular complexing agent and water, wherein the concentration of the metal compound in the mixture is preferably 0.001 to 0.15 g / ml, such as 0.01 to 0.1 g / ml, and reacting at 0 to 150° C., such as 70 to 90° C., for 0.5 to 24 h, such as 2 to 14 h;

[0014] (2) adding a small molecule alcohol such as ethanol or one or more of methanol, propanol, and ethylene glycol to the product of step (1); the mass ratio of water to alcohol in the resulting mixture is preferably 1:10 to 20:1;

[0015] (3) Separation such as filtration and drying.

[0016] According to the complex preparation method described in the above technical scheme, the modified metal compound is, for example, an oxide of a modified metal element and / or a modified metal element salt, and the modified metal element salt is, for example, one or more of a nitrate of a modified metal element, a chloride of a modified metal element, and a sulfate of a modified metal element; for example, the modified metal compound is one or more of manganese oxide, manganese salt, titanium oxide, titanium salt, barium oxide, barium salt, calcium oxide, and calcium salt.

[0017] The modified metal compound, macromolecular complexing agent and water are mixed. There is no special requirement for the order of the mixture. For example, the metal compound can be added to water under stirring, and then the complexing agent is added.

[0018] The macromolecular complexing agent is a complexing agent that can effectively complex with a modified metal selected from Ti, Ba, Ca, and Mn to form a macromolecular complex or a macromolecular complex cluster, and the formed macromolecular complex and the formed macromolecular complex cluster are difficult to enter the micropore channels of the catalyst, and are also not easy to enter the mesopore channels. The macromolecular complexing agent is, for example, one or more of polypyridine, EDTA, EDTA derivatives, macromolecular organic acids, macromolecular organic acid salts, NTA (nitrilotriacetic acid), EDDS (ethylenediamine disuccinic acid), PEI (polyetherimide), o-phenanthroline, pyrophosphate, and polyphosphate; the macromolecular complexing agent is preferably selected from ethylenediaminetetraacetic acid, ethylenediamine disuccinic acid, polyphosphoric acid and salts of the above acids, as well as one or more of polypyridine, diethanolamine, triethanolamine, and EDTA derivatives.

[0019] A method for preparing a catalytic cracking catalyst resistant to metal pollution, comprising:

[0020] (1) Providing catalytic cracking catalyst precursor microspheres (hereinafter referred to as catalyst precursor microspheres, precursor microspheres or first microspheres);

[0021] (2) providing a complex solution, wherein the complex solution comprises a complex formed by a modified metal ion and a complexing agent, and optionally contains an aluminum compound; the modified metal element is one or more of Ti, Ba, Ca, and Mn;

[0022] (3) contacting the catalytic cracking catalyst precursor microspheres with the complex solution, and optionally contacting with an aluminum compound solution or an aluminum-containing colloid to deposit aluminum on the outer surface of the catalyst precursor microspheres, to form catalytic cracking catalyst precursor microspheres having a surface layer containing a modified element, referred to as second microspheres; the aluminum introduced through the complex solution or the deposited aluminum is referred to as post-loaded aluminum, which can improve the bonding ability between the modified metal and the substrate, and the modified metal is not easy to fall off;

[0023] (4) drying the catalyst precursor microspheres having a surface layer containing a modified metal element, performing a first calcination, optionally treating them in a reducing environment such as a reducing gas, and optionally performing a second calcination treatment to obtain a catalytic cracking catalyst resistant to metal contamination.

[0024] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in the above technical solution, the molar ratio of the macromolecular complexing agent to the modified metal ion in the complex is preferably 0.5:1 to 10:1, for example 0.5 to 6:1, preferably 1 to 4:1.

[0025] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, in one embodiment, the complex solution is the complex solution obtained in step (1) of any of the above technical solutions for preparing the complex, or the complex solution is the complex solution formed by the complex provided by any of the above technical solutions for preparing the complex and water, or the solution formed by the complex obtained by the method for preparing the complex described in any of the above technical solutions and water. Optionally, the complex solution contains one or more of aluminum, phosphorus, boron, and rare earth compounds, and the phosphorus compound can be selected from one or more of phosphoric acid, pyrophosphoric acid, phosphorous acid, ammonium phosphate, and alkali metal phosphate; the rare earth compound can be selected from one or more of lanthanum and / or cerium chloride, nitrate, sulfate, hydroxide, and oxide, the boron compound can be selected from one or more of boric acid, boron oxide, tri-n-butyl borate, boron powder, and ammonium fluoroborate, and the aluminum compound is one or more of aluminum salts (such as chlorides, sulfates, nitrates), aluminum sol, phosphoaluminum colloid, and aluminum hydroxide.

[0026] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, the contact between the complex solution and the catalytic cracking catalyst precursor microspheres can be carried out by impregnation (for example, equal volume impregnation method, slurry impregnation method (a method in which the complex is adsorbed on the catalyst surface)), immersion, spraying (spray impregnation method is referred to as spraying method) or deposition method, preferably, spray impregnation method and equal volume impregnation method are adopted; the modified metal complex is loaded on the surface of the catalytic cracking catalyst precursor microspheres (forming a covering coating, referred to as coating or surface layer) through contact. A preferred embodiment is to spray the complex solution at high temperature, to evaporate the water in the solution sprayed on the catalyst precursor microspheres in time, to reduce the migration of macromolecular complexes to macropores and even to mesopores, which is beneficial to reduce the adverse effects of modified metals on the catalyst and improve the anti-metal pollution effect; an embodiment is to stir the catalytic cracking catalyst precursor microspheres while spraying the complex solution on the catalytic cracking catalyst precursor microspheres to promote uniform spraying.

[0027] The equal volume impregnation method, in one embodiment, is to mix a complex solution having a volume equal to the pore volume of the catalytic cracking catalyst precursor microspheres with the catalytic cracking catalyst precursor microspheres to adsorb the complex on the surface of the microspheres.

[0028] The spray impregnation method allows the complex solution to be evenly dispersed and sprayed onto the catalytic cracking catalyst precursor microspheres, and the spraying amount and spraying temperature are adjusted so that the water in the solution evaporates in time while spraying onto the surface; at the same time, the microspheres are turned over until the amount of complex sprayed makes the amount of metal in the obtained catalytic cracking catalyst meet the requirements. Preferably, the catalytic cracking catalyst precursor microspheres are contacted with the complex solution at a higher temperature so that the solvent in the complex solution sprayed onto the surface evaporates as quickly as possible.

[0029] The slurry impregnation method is to mix the catalytic cracking catalyst precursor microspheres with the complex solution and then precipitate with an alkaline precipitant. The complex can be adsorbed on the surface of the catalyst microspheres, and the addition of the alkaline precipitant can deposit the remaining modified metal complex on the catalyst surface during the stirring process.

[0030] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, in one embodiment, the catalyst precursor microspheres are contacted alternately with the complex solution and the aluminum compound dispersion to obtain catalyst precursor microspheres containing a modified metal element surface layer; wherein the molar ratio of aluminum to the modified metal is: 10:1 to 1:50, for example, 10:50 to 2:50; the alternating contact refers to the complex solution and the aluminum compound dispersion alternately contacting the catalyst precursor microspheres to deposit the modified metal and the aluminum compound on the surface of the microspheres, and the number of alternations is, for example, If it is 1 to 10 times, the amount of the complex solution contacted with the complex solution each time can be 10 to 100% by mass of the total amount of the complex solution, and the amount of the aluminum compound dispersion contacted with the aluminum compound dispersion each time can be 10 to 100% by mass of the total amount of the aluminum compound solution; preferably, after the contact with all the modified metal complex solutions is completed, at least one contact with the aluminum compound dispersion is carried out to improve the wear resistance of the surface layer; preferably, during spraying, the temperature of the catalytic cracking catalyst precursor microspheres is preferably 60 to 200°C, preferably 90 to 150°C.

[0031] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, wherein in step 3, the first microsphere is contacted with an aluminum compound dispersion to deposit aluminum on the surface of the first microsphere, and the aluminum compound dispersion is an aluminum compound solution and / or an aluminum-containing colloid. For example, the aluminum compound dispersion can be a solution containing Al ions such as an aluminum salt solution, or a solution containing an aluminum complex, or an aluminum-containing colloid such as an aluminum sol.

[0032] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical schemes, the temperature at which the complex solution is brought into contact with the catalytic cracking catalyst precursor microspheres (the temperature of the catalytic cracking catalyst precursor microspheres) in step (3) is 0 to 200°C, for example, 90 to 200°C, for example, 120 to 150°C, and the temperature of the sprayed complex solution is usually not more than 100°C, for example, 60-95°C.

[0033] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, in one embodiment, the catalytic cracking catalyst precursor microspheres include 10-60% by mass of molecular sieves, 10-50% by mass of binders and 0-70% by mass of clay. The molecular sieves are molecular sieves used in catalytic cracking catalysts, such as one or more of Y-type molecular sieves, MFI structure molecular sieves, IMF structure molecular sieves and BEA structure molecular sieves; the average particle size of the catalytic cracking catalyst precursor microspheres is preferably 60-80 microns, which can be measured by laser particle size method. Preferably, the sodium oxide content in the first microspheres does not exceed 0.4% by mass.

[0034] The catalytic cracking catalyst precursor microspheres can be existing fluidized catalytic cracking catalysts or unmodified microspherical intermediate products or semi-finished catalyst microspheres formed during the preparation of catalytic cracking catalysts. Catalytic cracking catalyst precursor microspheres can be purchased commercially or prepared according to existing methods, for example, they can be catalytic cracking catalyst microspheres synthesized by semi-synthetic methods or catalytic cracking catalyst microspheres synthesized by full synthetic methods. The unmodified microspherical intermediate products or semi-finished catalyst microspheres can be semi-finished catalyst microspheres that have not been de-sodiumed or modified by rare earth, P, ammonia, or acid washing. After the anti-pollution metal modification described in the present invention, they can be de-sodiumed, rare earth modified, phosphorus modified, ammonium ion modified, or hydrogen ion modified.

[0035] The fluidized catalytic cracking catalyst can be a semi-synthetic catalytic cracking catalyst microsphere or a fully synthetic catalytic cracking catalyst microsphere. The semi-synthetic catalytic cracking catalyst microsphere can be prepared by adding a zeolite component to a matrix slurry and spray drying to form a microsphere, or can be formed by first forming a microsphere through an in-situ crystallization technique, and then crystallizing the zeolite component in the microsphere itself to provide a microsphere containing a zeolite and a non-zeolite component. In particular, for the catalytic cracking catalyst microsphere prepared by the in-situ crystallization technique, after the modified metal is introduced into the method provided by the present invention, it can have a better anti-metal pollution effect.

[0036] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, the sodium oxide content in the catalytic cracking catalyst resistant to metal pollution does not exceed 0.3% by mass; when the sodium oxide content in the catalytic cracking catalyst is relatively high, the catalytic cracking catalyst is subjected to a sodium reduction treatment, and the catalytic cracking catalyst is subjected to a sodium reduction treatment, and the sodium reduction treatment can be selected from one of the following methods: Method 1, the catalytic cracking catalyst precursor microspheres are subjected to a sodium reduction treatment before spraying, and the mass content of Na2O in the catalytic cracking catalyst precursor microspheres is not greater than 0.4%, and the sodium oxide content is preferably not more than 0.3% by mass; Method 2, the sodium reduction treatment is performed after drying and / or calcination in step (4). The sodium reduction treatment can be carried out by water washing and / or ammonium exchange, which is well known to those skilled in the art.

[0037] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, the first calcination in step (4) is carried out at a temperature of 200-700°C, for example, a calcination temperature of 300-600°C, and a time of 0.1-3h, for example, a calcination time of 0.5-2.5h.

[0038] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, the second calcination in step (4) is carried out at a temperature of 300 to 750°C, such as 350 to 700°C, and for a time of 0.5 to 4 hours, such as 1 to 3 hours, so that the modified metal can be better combined with the catalyst surface matrix.

[0039] According to the method for preparing a catalytic cracking catalyst resistant to metal contamination described in any of the above technical solutions, wherein the treatment in step (4) under a reducing environment, such as a reducing atmosphere, has a treatment temperature of 350-700°C, such as 500-680°C or 580°C, 600°C or 650°C, and a treatment time of 0.5-6h, such as 0.5-4h. The reducing environment is in contact with a reducing agent, and can be a reducing atmosphere, such as an atmosphere containing one or more of hydrogen, CO, and H2S, or an environment in which one or more reducing agents such as S and C are present. When the modified metal includes Ca or Ba, the temperature of the treatment in the reducing environment, preferably the reducing atmosphere, is 550-700°C, such as 600-650°C, such as 600°C, 610°C, 620°C, 630°C or 640°C. When the modified metal includes Ti or Mn, the temperature of the treatment in the reducing environment, preferably the reducing atmosphere, is 600-700°C, such as 600°C, 610°C, 630°C, 650°C or 670°C, which can promote the combination with the surrounding matrix elements. Preferably, the treatment and the second calcination treatment are carried out in a reducing environment, preferably a reducing gas. The treatment in a reducing environment, preferably a reducing atmosphere, can promote the redistribution of the modified metal, can make the modified metal distribution better, the bonding is stronger, and the surface layer metal is less prone to wear.

[0040] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution as described in any of the above technical schemes, the concentration of the complex in the complex solution is 0.01-20 mass %, such as 0.5-15 mass %; the content of aluminum compound in the aluminum compound solution calculated as alumina is 0.1-30 mass %, such as 1-25 mass % or 2-20 mass %.

[0041] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution as described in any of the above technical schemes, the content of the modified metal element calculated as the element accounts for 0.01% to 1% of the total dry mass of the catalytic cracking catalyst resistant to metal pollution, and preferably, the content of the modified metal element calculated as the element accounts for 0.03% to 1.0%, for example 0.05% to 0.5%, of the total dry mass of the catalytic cracking catalyst resistant to metal pollution.

[0042] According to the method for preparing a catalytic cracking catalyst resistant to metal pollution described in any of the above technical solutions, the catalytic cracking catalyst resistant to metal pollution may also contain a second modifying element, and the second modifying element is, for example, B and / or P and / or rare earth. The introduction of rare earth, B and P includes but is not limited to in molecular sieves, matrix or clay, and the introduction method may be ion exchange introduction of molecular sieves or clay, or introduction into the slurry when the raw materials for preparing catalytic cracking catalyst precursor microspheres are mixed and slurried, or introduction by impregnation, ion exchange or deposition after molding.

[0043] In one embodiment, the second modifying element can be introduced by slurry impregnation, catalyst washing or deposition in the form of dilute acid and / or salt solution, or can be introduced into the catalytic cracking catalyst resistant to metal pollution in the form of oxide colloid. For example, the second element is introduced by spraying a compound containing the second modifying element. The compound of P is selected from one or more of phosphate aluminum colloid, phosphoric acid, pyrophosphoric acid, phosphorous acid, ammonium phosphate, and alkali metal phosphate; the rare earth compound is selected from one or more of lanthanum and / or cerium chloride, nitrate, hydroxide, sulfate, oxide, and the boron compound is such as one or more of boric acid, boric oxide, tri-n-butyl borate, boron powder, and ammonium fluoroborate.

[0044] The present invention further provides a catalytic cracking catalyst resistant to metal contamination, comprising microspheres with cracking activity and a surface layer containing modified metals on the surface of the microspheres, wherein the modified metals are one or more of Ti, Ba, Ca, and Mn, preferably Mn and / or Ti, and more preferably Mn.

[0045] According to the catalytic cracking catalyst resistant to metal pollution described in the above technical solution, the thickness of the modified metal surface layer (referred to as surface layer or coating) on ​​the catalyst surface is 0.1nm to 800nm, and the thickness of the surface layer is generally 1nm to 500nm. The boundary between the coating and the non-coating is at the position where the concentration of the modified metal drops sharply from the surface of the microsphere to the center of the microsphere, and the part away from the surface within the boundary is called the interior. The interior is the area within the boundary, usually, the area more than 100nm away from the boundary in the centripetal direction.

[0046] According to any of the above technical solutions, the catalytic cracking catalyst resistant to metal contamination, wherein the mass concentration of the modified metal in the modified metal surface layer is more than 50 times, for example, 50 to 1000 times, preferably more than 80 times, for example, 100 to 500 times, of the mass concentration inside the catalyst. The thickness of the metal ion annular distribution layer and the concentration change can be detected on the catalyst cross section by electron microscope EPMA micro-area analysis (linear analysis) method).

[0047] According to the metal-contamination-resistant catalytic cracking catalyst described in any of the above technical solutions, the mass ratio of the post-loaded aluminum to the modified metal in the surface layer is 10:1 to 1:50.

[0048] The metal-pollution-resistant catalytic cracking catalyst provided by the present invention may further contain one or more elements of rare earth, B and P as the second modifying element, and the positions of rare earth and phosphorus are not limited to the molecular sieve, matrix or clay. The rare earth metal elements preferably include those elements with atomic numbers of 57 to 71, such as La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu and mixtures of multiple elements thereof, for example, the rare earths are lanthanum and cerium.

[0049] Preferably, the content of the second modifying element (calculated as element) accounts for no more than 1% by mass, for example, 0 to 0.5% by mass, of the total mass of the catalytic cracking catalyst resistant to metal contamination on a dry basis.

[0050] The complex provided by the present invention is particularly suitable for preparing a catalytic cracking catalyst resistant to nickel pollution. The obtained catalyst can have a good nickel resistance effect when the amount of modified metal is low, thereby reducing the amount of modified metal. The method for preparing a catalytic cracking catalyst resistant to metal pollution provided by the present invention can prepare a metal pollution-resistant catalytic cracking catalyst having a surface layer containing a modified metal on the outer surface of the particle, and the catalyst can significantly improve the ability to resist metal pollution under the condition of a lower modified metal content. The obtained metal pollution-resistant catalytic cracking catalyst has a good nickel metal pollution resistance effect. In the case of nickel pollution, it is used for heavy oil cracking, has a good cracking product distribution, the ratio of hydrogen and methane in the product is low, and the hydrogen and coke yields can be reduced. In a preferred case, the conversion rate can be improved, and the distribution of high-value products can be optimized, such as increasing the LPG yield and / or increasing the gasoline yield and / or increasing the low-carbon olefin yield. The catalyst provided by the present invention can also have a certain vanadium pollution resistance effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is an electron probe microanalysis image of the Mn element of the metal-pollution-resistant catalytic cracking catalyst C1 prepared in Example 1. Electron probe EPMA microanalysis was used. In the Mn element distribution image, the highlighted area indicates a high manganese content, and it can be seen that Mn is mainly distributed on the outer surface of the catalyst. DETAILED DESCRIPTION

[0052] The present invention will be further described in the following examples, but the present invention is not limited thereto.

[0053] The catalyst precursor microspheres (catalytic cracking catalyst precursor microspheres) used in the examples and comparative examples are self-prepared catalytic cracking catalysts, and the preparation method thereof is the same as that in comparative example 1.

[0054] The surface layer thickness range measurement method of the embodiment: randomly measure the cross-section of 10 particles of the sample, and randomly measure three surface layer thicknesses of each particle cross-section to obtain the distribution range of the particle thickness.

[0055] Comparative Example 1

[0056] Take 200 parts by weight of pseudo-boehmite (dry basis, product of Shandong Aluminum Company), add deionized water and 24 parts by weight of hydrochloric acid with a concentration of 35% by weight, and beat to prepare acidified boehmite with a solid content of 12% by weight; then add 100 parts by weight of aluminum sol (dry basis), 340 parts by weight of kaolin (dry basis) and 360 parts by weight (dry basis) of DASY.2.0 molecular sieve (product of Qilu Branch of Sinopec Catalyst Co., Ltd.), stir for 0.5h, spray dry, calcine at 550°C for 2h, wash twice with a 2% by weight ammonium chloride solution, dry, and obtain basic catalytic cracking catalyst precursor microspheres, which are recorded as Cat-A. The basic chemical composition of Cat-A is shown in Table 1. The chemical composition is determined by X-ray fluorescence (XRF), see ASTM D7085-04 (2010) Standard Guide for the Determination of Chemical Elements in Fluidized Catalytic Cracking Catalysts - Guide for Determination by X-ray Fluorescence Spectrometry.

[0057] Table 1

[0058] Component name content Cl, %(W) 0.490 <![CDATA[Na2O,%(W)]]> 0.0458 <![CDATA[Al2O3,%(W)]]> 53.4 <![CDATA[SiO2,%(W)]]> 42.7 <![CDATA[P2O5,%(W)]]> 0.107 <![CDATA[SO3,%(W)]]> 1.67 <![CDATA[K2O,%(W)]]> 0.196 CaO, %(W) 0.057 <![CDATA[TiO2,%(W)]]> 0.288 <![CDATA[La2O3,%(W)]]> 0.309 <![CDATA[CeO2,%(W)]]> 0.607

[0059] In Table 1, % (W) refers to the mass percentage.

[0060] Example 1

[0061] Preparation of EDTA-Mn: In a 500 ml round bottom flask reactor, 19.79 g of manganese chloride tetrahydrate and 32.43 g of EDTA-2NH4 + Add to 100 ml of water, heat in a water bath at 80°C under magnetic stirring, adopt condensation reflux, and react for 3 hours to obtain a complex solution SOL1. After the reaction is completed, cool, add anhydrous ethanol to prepare a cold ethanol aqueous solution (the volume ratio of water to ethanol is 1:9) for precipitation, filter to obtain a precipitate, and then vacuum dry the product in a drying oven at 80°C for 12 hours to obtain 35.1 g of EDTA-Mn complex.

[0062] Preparation of AlCl3 solution: Take 2.68g AlCl3.6H2O and add it to 30g distilled water to make aluminum chloride solution;

[0063] 3.6g of EDTA-Mn complex was dissolved in 40g of distilled water to prepare complex solution SOL2, which was fully mixed with the aluminum chloride solution prepared above to obtain mixed solution SOL3, and then 100g of Cat-A (on a dry basis, the temperature was 95°C) was sprayed on the mixed solution SOL3 containing EDTA-Mn complex and aluminum chloride (the temperature was 80°C) by ultrasonic atomization method, and fully stirred while spraying, and then dried at 120°C for 2h, calcined at 500°C in air atmosphere for 1h, treated at 600°C in H2 atmosphere for 0.5h, and then calcined at 500°C in air atmosphere for 2h to obtain catalyst C1. The mass fraction of Mn in C1 is 0.5%. Among them, the thickness of the Mn-containing surface coating of C1 is 150-250nm, and the Mn concentration in the modified coating is 190 times the internal Mn concentration.

[0064] The cross-section of the catalyst microspheres was analyzed by EPMA electron microscope. The results are as follows: Figure 1 As shown, the modified metal distribution is almost invisible inside. The analysis method for detecting the internal Mn content by EPMA micro-analysis is as follows: After cutting the catalyst particles, take any particle, take a diameter line on the cross section, and perform Mn element line scanning analysis. The thickness of the modified metal coating in the cross section and the modified metal concentration in the coating and the interior (i.e., the area more than 100 microns away from the non-coated edge of the particle) can be measured.

[0065] Example 2

[0066] Take 1.88g of commercial EDTA-NaTi and dissolve it in 50g of distilled water to prepare a Ti-containing complexing agent solution, and take 2.68g of AlCl3.6H2O and dissolve it in 50g of distilled water to prepare an aluminum chloride solution. 100g CAT-B on a dry basis was placed in a stirring heating tank at 90℃~110℃, and firstly, 10g aluminum chloride solution was used for atomization spraying, and the mixture was dried while stirring; then, 10g Ti-containing complexing agent solution was used for spraying, and two equal solutions were used for Al-Ti-Al-Ti treatment in sequence, and both solutions needed to be sprayed and stirred until both solutions were completely sprayed, and then the mixture was heated in a stirring tumbling heating tank for 1h, and then calcined in air at 600℃ for 1h, treated at 600℃ in an atmosphere containing 30vol% H2 and 70vol% N2 for 3h, and then calcined at 600℃ in an air atmosphere for 1h, and then washed with 2% ammonium sulfate solution until the Na content was less than 0.3% by mass, and then dried to obtain catalyst C2. The Ti mass fraction of C2 was 0.3%, and the sodium oxide sodium content was 0.2% by mass. Among them, the thickness of the Ti-containing coating of C2 is 200-300 nm, and the Ti concentration in the modified coating is 287 times that of the internal Ti concentration.

[0067] Example 3

[0068] Preparation of EDDS-Ba: In a 500ml round-bottom flask reactor, 28.8g of barium sulfate and 40.12g of trisodium ethylenediamine epoxysuccinate were added to 150ml of water, heated in a water bath at 80°C under magnetic stirring, and condensed and refluxed for 2h. After the reaction, the mixture was cooled, anhydrous ethanol was added to prepare a cold ethanol aqueous solution (the volume ratio of water to ethanol was 1:9) for precipitation, and the precipitate was obtained by filtration. The product was then vacuum dried in a drying oven at 80°C for 12h, and about 53g of EDDS-Ba complex was obtained.

[0069] 1.64g of the above EDDS-Ba complex was dissolved in 40g of distilled water to prepare EDDS-Ba solution, and then 100g of Cat-A (on a dry basis) was mixed and stirred to perform equal volume impregnation, and then dried at 120°C for 2h, calcined at 400°C in air atmosphere for 1h, and then treated in carbon monoxide at 600°C for 0.5h, and then calcined in air atmosphere at 600°C for 1h, and then washed with ammonium sulfate solution to obtain catalyst C3. The Ba mass fraction of C3 is 0.35%. The sodium oxide content is 0.15% by mass, wherein the Ba-containing coating thickness of C3 is 250-300nm, and the Ba concentration in the modified coating is 300 times the internal Ba concentration.

[0070] Example 4

[0071] The catalyst C4 was prepared by the method of reference example 1, except that the prepared EDTA-Mn complex solution SOL2 was replaced by the complex solution SOL1, and the mass fraction of Mn was about 0.5%. The thickness of the Mn coating was about 200-300 nm, and the Mn concentration in the modified coating was 61 times the Mn content in the interior.

[0072] Example 5

[0073] Reference is made to the method of Example 1, except that the calcination treatment in a hydrogen atmosphere is not performed, and is denoted as C5.

[0074] Comparative Example 2

[0075] Referring to the method of Example 1, the EDTA-Mn complexing agent solution was not sprayed and loaded. Only 100 g of Cat-A was fully mixed with the aluminum chloride solution prepared in Example 1, and then dried at 120°C for 2 h, and then calcined at 500°C for 1 h-500°C for reduction for 0.5 h-500°C for calcination for 1 h to obtain catalyst D2.

[0076] Comparative Example 3

[0077] 16.2 kg of aluminum sol was added to 5.4 kg of decationized water and mixed evenly. 7.1 kg of rectorite was added under stirring. The mixture was heated to 60° C. and stirred for 30 minutes. Then, 1138 g of manganese chloride (MnCl2·4H2O, produced by Beijing Chemical Reagent Company) was added. After stirring for 60 minutes, a slurry with a solid content of 35% by mass was obtained, which was recorded as T1.

[0078] Take 200g (on a dry basis) of Shandong pseudo-boehmite, add appropriate amount of deionized water and 24g of hydrochloric acid, and beat to prepare an acidified boehmite solution with a solid content of 12%; then add 100g (on a dry basis) of aluminum sol, 270g of kaolin (on a dry basis), 360g of DASY.2.0 (on a dry basis), and 70g of T1 (on a dry basis), fully homogenize and stir for 0.5h, spray dry, further roast, and wash with ammonium sulfate to obtain a catalyst D3 with a Mn content of about 0.7% by mass. Mn metal is dispersed in the catalyst.

[0079] Comparative Example 4

[0080] In a 3-liter (hereinafter liter is referred to as "L" and milliliter is referred to as "mL") glass beaker containing 1,000 mL of distilled purified water, 271.9 g of manganese sulfate pentahydrate was dissolved, followed by stirring with a magnetic stirrer for 15 minutes to prepare a solution A, the pH of the solution A being 4.5;

[0081] In a 3-L glass beaker containing 1,000 mL of distilled purified water, 125 g of aluminum sulfate 18hydrate was dissolved, followed by stirring with a magnetic stirrer for 15 minutes to prepare a solution B, the pH of the solution B being 1.6;

[0082] Solution A and Solution B were mixed in a 5-L glass beaker, heated to 80°C and stirred with a magnetic stirrer to prepare Solution C;

[0083] In a 5-L glass beaker containing 1,000 mL of distilled purified water, 113.8 g of sodium carbonate was dissolved, followed by heating to 80° C. and stirring with an ultra disperser for 15 minutes to prepare a solution D, the pH of the solution D being 11.47;

[0084] While stirring solution D with a superdisperser, solution C was gradually added thereto with a feed pump. During the operation, ammonia water was also added to maintain the pH of the solution mixture at 9;

[0085] The solution mixture was aged at 80° C. for 3 hours with stirring to obtain a metal compound;

[0086] After aging was terminated, the solution was filtered through a Buchner funnel. To the separated slurry (metal compound), 2 L of distilled purified water heated to 80° C. was added, and the obtained mixture was stirred and filtered; the operation was repeated twice to perform washing;

[0087] drying the slurry separated by filtration at 100° C. for about 24 hours to obtain a metal compound;

[0088] The metal compound obtained by grinding the dried metal compound to a particle size of 15 μm or less is referred to as MC-1 (Mn—Al—CO 3 ).

[0089] Take 200g (on a dry basis) of pseudo-boehmite, add appropriate amount of deionized water and 24g of hydrochloric acid, and slurry to prepare an acidified boehmite solution with a solid content of 12%; then add 100g (on a dry basis) of aluminum sol, 340g of kaolin (on a dry basis) and 360g of DASY.2.0 (on a dry basis), as well as 10g (on a dry basis) of MC-1, and after fully homogenizing and stirring for 0.5h, spray drying, further calcination, and ammonium washing, the catalyst D4 with a Mn content of about 0.8% by mass is obtained.

[0090] Comparative Example 5

[0091] The catalyst D5 was prepared by the method of reference Example 3, except that the EDDS-Ba complex solution was sprayed with a barium sulfate solution of the same molar concentration instead of the EDDS-Ba complex solution, and the mass fraction of Ba was about 0.4%. Among them, D5 had no modified metal coating with a clear boundary line, and the modified metal gradually decreased from the surface layer, and no obvious coating distribution appeared.

[0092] Embodiments 6 to 10

[0093] This example illustrates the metal resistance of the heavy oil cracking catalyst provided by the present invention.

[0094] Catalysts C1, C2, C3, C4, and C5 were respectively subjected to the cyclic contamination method on the ACE D100 device, and nickel cyclohexaneate and vanadium cyclohexaneate were dissolved in the distillate oil at a mass ratio of 5:2 for multiple cyclic reactions until the Ni on the catalyst was about 4500ppm (mass) and V was 1800ppm (mass). The samples after cyclic contamination were numbered C1w, C2w, C3w, C4w, and C5w. Samples C1w to C5w were then aged for 12 hours at 100% steam in a fixed bed at 800°C, and then evaluated using an ACE fluidized bed device. The ACE-evaluated crude oil properties are shown in Table 2, and the evaluation conditions and results are shown in Table 3.

[0095] Comparative Examples 6 to 10

[0096] This example illustrates the metal resistance of the heavy oil cracking catalyst provided by the present invention.

[0097] Catalysts Cat-A, D2, D3, D4, and D5 were respectively subjected to the cyclic contamination method on the ACE D100 device, and nickel cyclohexaneate and vanadium cyclohexaneate were dissolved into the distillate oil at a mass ratio of 5:2 for multiple cyclic reactions until the Ni on the catalyst was about 4500ppm by mass and the V was 1500ppm by mass. The sample numbers after cyclic contamination were Cat-Aw, D2w, D3w, D4w, and D5w, respectively. Then the samples Cat-Aw, D2w, D3w, and D4w were aged for 12 hours at 100% steam at 800°C in a fixed bed, and then evaluated using an ACE fluidized bed device. The ACE-evaluated crude oil properties are shown in Table 2, and the evaluation conditions and results are shown in Table 4.

[0098] Table 2

[0099]

[0100] Table 3

[0101] Catalyst name C1W C2 C3W C4w C5W Cracking reaction temperature,℃ 500.0 500.0 500.0 500.0 500.0 Agent to oil ratio, wt / wt 4.02 4.02 4.02 4.02 4.02 Yield, wt% Dry gas 2.09 2.19 2.20 2.04 2.07 Liquefied gas 13.54 12.63 12.36 12.95 13.58 Coke 10.32 11.33 10.64 10.52 10.37 gasoline 45.43 44.28 45.12 43.05 45.32 diesel fuel 18.87 19.04 19.07 20.21 18.62 heavy oil 9.75 10.53 10.61 11.23 10.04 hydrogen 0.30 0.39 0.38 0.36 0.32 Methane 0.87 0.91 0.91 0.84 0.89 Ethane 0.47 0.46 0.47 0.43 0.42 Ethylene 0.45 0.43 0.44 0.41 0.44 Propane 0.98 0.81 0.91 0.87 0.88 Propylene 3.74 3.68 3.68 3.70 3.70 n-Butane 0.83 0.66 0.70 0.73 0.79 Isobutane 3.59 2.95 3.14 3.22 3.63 C4 olefins 4.40 4.53 3.93 4.43 4.58 1-Butene 0.93 0.92 0.83 0.92 0.89 Isobutylene 1.20 1.35 1.12 1.27 1.41 c-2-Butene 0.92 0.94 0.81 0.92 0.95 t-2-Butene 1.35 1.32 1.17 1.32 1.33 Conversion rate, wt% 71.38 70.43 70.32 68.56 71.34 Hydrogen to methane ratio (mol ratio) 2.76 3.42 3.34 2.97 2.87

[0102] Table 4

[0103] Catalyst name Cat-Aw dW 3W D4W 5W Cracking reaction temperature,℃ 500.0 500.0 500.0 500.0 500.0 Agent-oil ratio, wt / wt 4.02 4.02 4.02 4.02 4.02 Yield wt% Dry gas 2.29 2.23 2.21 2.21 1.92 Liquefied gas 12.03 12.06 12.78 12.47 11.08 Coke 11.62 11.49 10.85 11.57 9.31 gasoline 43.23 43.31 41.55 43.25 41.42 diesel fuel 19.57 19.48 20.75 19.11 23.85 heavy oil 11.26 11.43 11.86 11.39 12.42 hydrogen 0.56 0.51 0.48 0.47 0.39 Methane 0.86 0.89 0.85 0.87 0.79 Ethane 0.44 0.43 0.46 0.46 0.39 Ethylene 0.43 0.40 0.42 0.41 0.35 Propane 0.81 0.81 0.93 0.92 0.74 Propylene 3.66 3.55 3.61 3.63 3.29 n-Butane 0.62 0.63 0.76 0.76 0.56 Isobutane 2.88 2.78 3.23 2.90 2.55 C4 olefins 4.06 4.29 4.25 4.26 3.95 1-Butene 0.83 0.87 0.91 0.89 0.84 Isobutylene 1.22 1.30 1.20 1.18 1.06 c-2-Butene 0.83 0.88 0.81 0.89 0.83 t-2-Butene 1.18 1.24 1.33 1.30 1.22 Conversion rate, wt% 69.17 69.09 67.39 69.50 63.73 Hydrogen to methane ratio (mol ratio) 5.21 4.58 4.52 4.32 3.95

[0104] As can be seen from Table 3, the ACE evaluation reaction result of C5w is similar to that of C1w, but after C1 and C5 were purged for 4 hours in a straight tube wear device (see NB / SH / T 0964-2017 Straight tube method for determination of wear index of catalytic cracking catalysts), the Mn content was tested by XRF. Compared with before the wear and purge test, the Mn mass fraction decreased by about 16% (multiple measurements), while the Mn loss rate of C1 was less than 9% after 4 hours of wear in the straight tube wear device. This shows that the method of the present invention adopts a reduction step, and the obtained catalyst has a stronger nickel metal capacity, and is less likely to cause nickel metal loss in actual catalytic cracking conditions, which is conducive to maintaining a better effect.

[0105] It can be seen from Tables 3 and 4 that, relative to the Cat-Aw catalyst that does not contain modified metals, the catalyst provided by the present invention has lower hydrogen and coke yields after contamination, and can significantly reduce the hydrogen-methane ratio. When the content of modified metal oxides is equivalent or lower, compared with catalysts prepared by other methods, the catalytic cracking catalyst provided by the present invention has lower dry gas and hydrogen-methane ratios when containing contaminated metals, and the hydrogen yield is lower. In addition, the metal pollution-resistant catalyst provided by the present invention can and has a higher heavy oil conversion capacity. In a preferred case, for example, when the modified metal element is Mn, the catalytic cracking catalyst provided by the present invention can have a higher light olefin yield and a higher conversion rate with a lower hydrogen-methane ratio.

Claims

1. A complex for improving the metal resistance of catalytic cracking catalysts, characterized in that: It comprises a modified metal ion and a complexing agent, wherein the molar ratio of the complexing agent to the modified metal ion is 0.5:1 to 10:1, the modified metal is one or more of Ti, Mn, Ba, and Ca, and the complexing agent is a macromolecular complexing agent; The macromolecular complexing agent is one or more of polypyridine, EDTA, EDTA derivatives, NTA, EDDS, PEI, o-phenanthroline, pyrophosphate, and polyphosphate; The macromolecular complexing agent in the complex forms a complex and / or complex cluster with a kinetic diameter of not less than 5 nm with the metal; The preparation method of the complex comprises the following steps: 1) Mix the modified metal compound, macromolecular complexing agent and water, wherein the concentration of the metal compound in the mixture is 0.001-0.15 g / mL, the reaction temperature is 0-150°C, and the reaction time is 0.5-24 h; 2) adding a small molecule alcohol to the product of step 1); the mass ratio of water to alcohol in the obtained mixture is 1:10 to 20:1; 3) Separation and drying.

2. The complex according to claim 1, characterized in that The molar ratio of the macromolecular complexing agent molecules to the metal ions is 0.5-6:

1.

3. The complex according to claim 2, characterized in that The molar ratio of the macromolecular complexing agent molecules to the metal ions is 1-4:

1.

4. A method for preparing the complex according to claim 1, 2 or 3, comprising the following steps: 1) Mixing a modified metal compound, a macromolecular complexing agent and water, wherein the concentration of the metal compound in the mixture is 0.001-0.15 g / mL, the reaction temperature is 0-150° C., and the reaction time is 0.5-24 h; the macromolecular complexing agent and the metal in the complex form a complex and / or complex cluster with a kinetic diameter of 5-100 nm; 2) adding a small molecule alcohol to the product of step 1); the mass ratio of water to alcohol in the obtained mixture is 1:10 to 20:1; 3) Separation and drying.

5. The method for preparing the complex according to claim 4, characterized in that: The modified metal compound is an oxide of the modified metal element and / or a salt of the modified metal element. The modified metal element salt includes one or more of the nitrate, chloride and sulfate of the modified metal element.

6. The method for preparing the complex according to claim 5, characterized in that: The macromolecular complexing agent is one or more of ethylenediaminetetraacetic acid, ethylenediamine disuccinic acid, polyphosphoric acid and salts of the above acids, polypyridine, diethanolamine, and triethanolamine. In step 1), the concentration of the metal compound in the mixture is 0.01-0.1 g / mL, and the reaction is carried out at 70-90° C. for 2-14 hours.

7. The method for preparing the complex according to claim 5, characterized in that: The small molecule alcohol is one or more of ethanol, methanol, propanol and ethylene glycol.

8. A method for preparing a catalytic cracking catalyst resistant to metal pollution, comprising: (1) Providing catalytic cracking catalyst precursor microspheres; (2) Providing a complex solution, wherein the complex solution comprises a complex formed by a modified metal ion and a complexing agent, and optionally contains an aluminum compound; the modified metal element is one or more of Ti, Ba, Ca, and Mn, and the complexing agent is a macromolecular complexing agent; the molar ratio of the complexing agent to the modified metal ion is 0.5:1 to 10:1; the concentration of the complex in the complex solution is 0.01 to 20% by mass; and the macromolecular complexing agent is one or more of polypyridine, EDTA, EDTA derivatives, NTA, EDDS, PEI, o-phenanthroline, pyrophosphate, and polyphosphate; The complex solution preparation method comprises: mixing a modified metal compound, a macromolecular complexing agent and water, wherein the concentration of the metal compound in the mixture is 0.001-0.15 g / mL, the reaction temperature is 0-150° C., and the reaction time is 0.5-24 h; (3) contacting the catalytic cracking catalyst precursor microspheres with the complex solution, and optionally with an aluminum compound solution or an aluminum-containing colloid, to obtain catalyst precursor microspheres having a surface layer containing a modified metal element; (4) Drying the catalyst precursor microspheres having a surface layer containing a modified metal element, performing a first calcination, optionally treating in a reducing environment, and optionally performing a second calcination to obtain a catalytic cracking catalyst resistant to metal contamination.

9. The preparation method according to claim 8, characterized in that: The molar ratio of the macromolecular complexing agent to the metal ion is 0.5-6:

1.

10. The preparation method according to claim 8, characterized in that: The complex solution preparation method comprises the following steps: 1) Mix the modified metal compound, macromolecular complexing agent and water, wherein the concentration of the metal compound in the mixture is 0.001-0.15 g / mL, the reaction temperature is 0-150°C, and the reaction time is 0.5-24 h; 2) adding a small molecule alcohol to the product of step 1); the mass ratio of water to alcohol in the obtained mixture is 1:10 to 20:1; 3) Separate, dry and dissolve in water.

11. The preparation method according to claim 10, characterized in that: The modified metal compound is an oxide of a modified metal element and / or a salt of a modified metal element, and the modified metal element salt includes one or more of a nitrate, a chloride and a sulfate of the modified metal element; The macromolecular complexing agent is one or more of ethylenediaminetetraacetic acid, ethylenediamine disuccinic acid, polyphosphoric acid and salts of the above acids, polypyridine, diethanolamine, and triethanolamine; The small molecule alcohol is one or more of ethanol, methanol, propanol and ethylene glycol.

12. The method for preparing a catalytic cracking catalyst resistant to metal pollution according to claim 9, characterized in that: The molar ratio of the macromolecular complexing agent to the modified metal ion in the complex is 1-4:

1.

13. The preparation method according to claim 8, characterized in that: The complex solution contains one or more of aluminum, phosphorus, boron and rare earth compounds; The complex solution is contacted with the catalytic cracking catalyst precursor microspheres by dipping, leaching, spraying or deposition; In step (3), the catalyst precursor microspheres are brought into contact with the complex solution and the aluminum compound dispersion to obtain catalyst precursor microspheres containing a modified metal element surface layer; The molar ratio of aluminum to the modified metal is 10:1 to 1:50; the content of the aluminum compound in the aluminum compound dispersion is 0.1 to 30% by mass in terms of aluminum oxide; The temperature for contacting the complex solution with the catalytic cracking catalyst precursor microspheres in step (3) is 0-200°C.

14. The preparation method according to claim 13, characterized in that: In step (3), the molar ratio of aluminum to modified metal is 10:50 to 2:

50.

15. The preparation method according to claim 13, characterized in that: The temperature for contacting the complex solution with the catalytic cracking catalyst precursor microspheres in step (3) is 90-200°C.

16. The preparation method according to claim 8, characterized in that: The first calcination in step (4) is carried out at a temperature of 200-700°C for a time of 0.1-3 h. The second calcination in step (4) is carried out at a temperature of 300-750°C for a time of 0.5-4 h. The treatment in a reducing environment in step (4) is carried out at a temperature of 350-700°C for a time of 0.5-6 h.

17. The preparation method according to claim 16, characterized in that: The first calcination in step (4) is carried out at a temperature of 300-600°C for a time of 0.5-2.5 h; the second calcination in step (4) is carried out at a temperature of 350-700°C for a time of 1-3 h; the treatment in a reducing environment in step (4) is carried out at a temperature of 500-680°C for a treatment time of 0.5-6 h.

18. The preparation method according to claim 8, characterized in that: The reducing environment is under reducing gas.

19. The method according to claim 8, characterized in that The catalytic cracking catalyst precursor microspheres include 10-60 mass % of molecular sieve, 10-50 mass % of binder and 0-70 mass % of clay; The catalytic cracking catalyst precursor microspheres are fully synthetic catalytic cracking catalyst microspheres, semi-synthetic catalytic cracking catalyst microspheres prepared by adding zeolite components to matrix slurry and spray drying, or catalytic cracking catalyst microspheres prepared by in-situ crystallization technology.

20. The preparation method according to claim 8, characterized in that: The concentration of the complex in the complex solution is 1 to 15% by mass; the content of the aluminum compound in the aluminum compound dispersion calculated as aluminum oxide is 2 to 20% by mass.

21. The catalytic cracking catalyst resistant to metal contamination obtained by the preparation method of the catalytic cracking catalyst resistant to metal contamination according to any one of claims 8 to 20 comprises microspheres with cracking activity and a surface layer containing a modified metal on the surface of the microspheres, wherein the modified metal is one or more of Ti, Ba, Ca, and Mn, and the thickness of the surface layer containing the modified metal on the catalyst surface is 0.1 nm to 800 nm.

22. The catalytic cracking catalyst resistant to metal contamination according to claim 21, characterized in that: The thickness of the surface layer containing modified metal is 1nm~500nm.

23. The catalytic cracking catalyst resistant to metal contamination according to claim 21, characterized in that: The mass concentration of the modified metal in the modified metal surface layer is more than 50 times the mass concentration inside the catalyst.

24. The catalytic cracking catalyst resistant to metal contamination according to claim 21, characterized in that: The mass ratio of the post-loaded aluminum to the modified metal in the surface layer is 10:1 to 1:

50.

25. The catalytic cracking catalyst resistant to metal contamination according to claim 21, characterized in that: In the catalytic cracking catalyst resistant to metal pollution, the content of modified metal elements in terms of elements accounts for 0.01% to 1% of the total dry mass of the catalytic cracking catalyst resistant to metal pollution; the content of sodium oxide in the catalytic cracking catalyst resistant to metal pollution does not exceed 0.3% by mass.

26. The catalytic cracking catalyst resistant to metal contamination according to claim 25, characterized in that: In the catalytic cracking catalyst resistant to metal contamination, the content of the modified metal element, calculated as the element, accounts for 0.05% to 0.5% of the total mass of the catalytic cracking catalyst resistant to metal contamination on a dry basis.

27. The catalytic cracking catalyst resistant to metal contamination according to claim 21, characterized in that: The metal-pollution-resistant catalytic cracking catalyst also contains a second modifying element, which is B and / or P and / or rare earth; the content of the second modifying element, calculated as an element, accounts for no more than 1% by mass of the total dry mass of the metal-pollution-resistant catalytic cracking catalyst.

Citation Information

Patent Citations

  • Catalytic cracking catalyst containing modified molecular sieve and preparation method of catalytic cracking catalyst

    CN105562060A

  • Heavy oil cracking catalyst and preparation method thereof

    CN105582973A

  • Cracking catalyst and preparation method thereof

    CN105618110A

  • Preparation method of catalytic cracking catalyst

    CN106890664A

  • Preparation method for rare earth-containing catalytic cracking catalyst

    CN106890675A