A method for preparing high elastic modulus dense cordierite ceramic material

By adding GeO2-SnO2 amorphous additives to cordierite ceramic materials and adjusting the composition and sintering conditions, cordierite ceramics with high density and low thermal expansion coefficient were prepared, solving the precision error problem of the lithography machine's moving platform and achieving the stability and precision requirements of high-precision lithography machines.

CN115959894BActive Publication Date: 2024-11-01JINGDEZHEN CERAMIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310138589.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-20
Publication Date
2024-11-01
Estimated Expiration
2043-02-20

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare cordierite ceramic materials with high density and low coefficient of thermal expansion, resulting in large accuracy errors of the lithography machine's moving platform under temperature changes and stress, and making it difficult to meet the performance requirements of high-precision lithography machines.

Method used

High-elasticity, dense cordierite ceramic materials were prepared by adding GeO2-SnO2 amorphous additives to adjust the composition and sintering conditions of cordierite ceramic raw materials. The process included ball milling, slip casting, and high-temperature firing, which controlled the thermal expansion coefficient and mechanical strength of the material.

Benefits of technology

Cordierite ceramic materials with high mechanical strength, low water absorption and low coefficient of thermal expansion were prepared to meet the high precision requirements of precision equipment such as lithography machines, and improve the overlay accuracy and stability of lithography machines.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for preparing a high elastic modulus dense cordierite ceramic material, comprising the following steps: Step 1: preparing GeO 2 ‑SnO 2 System amorphous additives; Step 2: By weight percentage: MgO 11-16%, Al 2 O 3 29~37%, SiO 2 51-59% of cordierite ceramic raw material is configured, and then the amorphous additive, tap water, and organic debonding agent obtained in step 1 are added, and after weighing, mixing, ball milling, screening, slip casting, green body drying, high-temperature firing, and cooling, a high elastic modulus dense cordierite ceramic material is obtained. The material has high density, low thermal expansion coefficient, and high elastic modulus. The low thermal expansion can ensure that the dimensional accuracy of the mobile platform is not affected by ambient temperature fluctuations and temperature changes caused during processing, and the high modulus can ensure that the mobile platform will not deform even if subjected to a large external force, thereby ensuring the working accuracy of the mobile platform, and therefore has broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new inorganic materials, and in particular to a method for preparing a dense cordierite ceramic material with high elastic modulus. Background Art

[0002] The mobile platform is a core component of high-precision equipment such as lithography machines. Its motion accuracy and repeatability directly determine the quality of the produced chips, and the material system design of the mobile platform is the key to high precision and high speed of equipment such as lithography machines. Since the ambient temperature of the lithography machine will inevitably fluctuate to a certain extent, and the temperature of each component of the machine will inevitably rise to different degrees after a long period of operation, although the absolute value of the temperature change is not large, for lithography machines with an overlay accuracy requirement of 1 to 2nm, a slight temperature change may cause a slight change in the size of the mobile platform itself due to thermal expansion and contraction, thereby causing serious errors in the overlay accuracy of the lithography machine. Therefore, the selection of materials with low thermal expansion coefficients for the moving platform is the key to ensuring its overlay accuracy. In addition, during the processing of the lithography machine, it is inevitable that some parts will form internal stress due to various irresistible forces. If the elastic modulus of the material used for the mobile platform is small, the material may produce a certain degree of displacement under a small stress. This displacement is undoubtedly fatal to high-precision lithography machines. Therefore, when selecting the material system of the mobile platform, it is necessary to ensure that the selected material has a large elastic modulus.

[0003] At present, ASML lithography machines in the Netherlands almost monopolize the domestic and foreign high-end chip equipment market. The materials used in the mobile platform have undergone a transformation from quartz glass, microcrystalline glass to cordierite ceramics. Although quartz glass and microcrystalline glass such as Zerodur have very low thermal expansion coefficients, their elastic moduli are all below 100 GPa, while cordierite ceramics have an elastic modulus of up to about 150 GPa while having a low thermal expansion coefficient. At the same time, the large amount of glass phase in glass and microcrystalline glass materials is easily corroded during EUV ion etching, causing platform wear and affecting overlay accuracy. Therefore, cordierite ceramics are the most ideal material for mobile platforms. At present, the materials used for mobile platforms of domestic lithography machines are mainly SiC materials. Although SiC has an elastic modulus of up to 400 GPa, its thermal expansion coefficient is high, which makes it difficult to meet the strict requirements of lithography machines for precision errors caused by temperature changes, and can only be used for the design and manufacture of mid- and low-end lithography machines.

[0004] Cordierite ceramics are a typical low thermal expansion ceramic material. Due to the anisotropy of the expansion coefficient of cordierite crystals, microcracks are inevitable during the cooling process after high temperature firing. Therefore, low expansion cordierite ceramic materials often have low strength. In addition, cordierite is based on MgO-Al 2 O 3 -SiO2 The ternary system ceramics do not have alkali metal oxides as flux components in the theoretical composition, which results in a very high sintering temperature (about 1430°C), which is very close to its melting point of 1460°C. Therefore, the sintering temperature range of cordierite ceramics is very narrow. At the same time, due to the absence of a liquid phase formed by a flux, it is also very difficult to obtain dense cordierite ceramics. Even if non-dense cordierite ceramics are processed and polished with high precision, it is impossible to obtain high-quality surface quality due to the presence of micropores in the structure, and it is difficult to meet the stringent requirements of the 0.1nm root mean square roughness of the mirror substrate material of the lithography mobile platform. Adding flux components such as alkali metal oxides to form a liquid phase in the sintering process is the main way to achieve ceramic densification. However, the added flux components will cause the thermal expansion coefficient of cordierite ceramic materials to increase significantly, thereby losing the advantage of being a low expansion material. Therefore, studying the preparation technology of high-density, low thermal expansion cordierite ceramics is of great significance to the design and manufacture of precision equipment such as lithography mobile platforms. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a dense cordierite ceramic material with high elastic modulus, which has simple process, low cost and can be applied on a large scale.

[0006] The technical solution of the present invention is: a method for preparing a dense cordierite ceramic material with a high elastic modulus, characterized by comprising the following steps:

[0007] Step 1: Preparation of GeO 2 -SnO 2 System amorphous additives;

[0008] Step 2: By weight percentage: MgO 11-16%, Al 2 O 3 29~37%, SiO 2 51-59% of cordierite ceramic raw material is configured, and then the amorphous additive, tap water and organic debonding agent obtained in step 1 are added, and after weighing, mixing, ball milling, screening, slip casting, green body drying, high temperature firing and cooling, a high elastic modulus dense cordierite ceramic material is obtained.

[0009] In step 1, GeO 2 -SnO 2 The preparation steps of the amorphous additive system are as follows: by weight percentage: GeO 2 55~78%, SnO 2 22~45%, after the raw materials are evenly mixed, they are loaded into a corundum crucible or a quartz crucible, placed in a high-temperature electric furnace and heated from room temperature to 1450~1550℃ and kept warm for 1~3h to obtain a uniform melt, and the melt is water quenched, ball milled, dried, and passed through a 200~300 mesh standard sieve to obtain amorphous micropowder.

[0010] In the second step, MgO in the cordierite ceramic raw material is introduced as magnesium oxide, Al 2 O 3 Introduced with kaolin, SiO 2 Introduced with kaolin and quartz.

[0011] The K in kaolin 2 O、Na 2 The total weight content of O is less than 0.1wt%, Fe 2 O 3 With TiO 2 The sum of the weights of the color-developing substances is less than 0.2wt%.

[0012] In the step 2, the amount of the amorphous additive added is 1-6wt% of the weight of the cordierite ceramic raw material, the amount of tap water added is 30-35wt% of the total weight of the raw material and water, and the amount of the organic dissolving agent added is 0.3-0.5wt% of the total weight of the raw material and water.

[0013] The ball mill used in the ball milling process of step 2 is ZrO 2 The amount added is 2 to 3 times the total mass of raw materials and water; the ball milling time is 1 to 3 hours.

[0014] The mesh size of the sieve in the second step of the sieving process is 100-200 meshes; the temperature in the green body drying process is 60-80° C. and the drying time is 2-6 hours.

[0015] The system of the high temperature firing process in step 2 is to heat to 1290-1360° C. at a heating rate of 3-20° C. / min and keep the temperature for 1-3 hours.

[0016] The high-performance cordierite ceramic material obtained in step 2 has a mechanical strength of 69-156 MPa, an elastic modulus of 152-173 GPa, an absorptivity of 0.01-0.02 wt%, a thermal expansion coefficient of 0.9-1.6×10 -6 ℃ -1 .

[0017] The high-performance cordierite ceramic material obtained in step 2 can be applied to mobile platforms of precision equipment such as photolithography machines.

[0018] The present invention has the following beneficial effects:

[0019] (1) Due to GeO 2、 SnO 2 With SiO 2 They are all in Group IV of the periodic table and have similar molecular structures and physical and chemical properties. Therefore, they can replace [SiO 4] without affecting the thermal expansion properties of the cordierite crystal.

[0020] (2) GeO 2 The melting point of SnO is 1086℃. 2 The melting point is 1630℃, which is higher than SiO 2 The melting point of GeO is 1710℃, which is lower than that of 2 -SnO 2 The relative content of the two in the binary system can obtain amorphous materials with different low eutectic temperatures, so that cordierite ceramics can form a certain amount of liquid phase under relatively low temperature conditions during the sintering process, accelerate the mass transfer during the sintering process, and then promote the densification of cordierite ceramics, making cordierite ceramics have a very low water absorption rate.

[0021] (3) The prepared cordierite ceramic material has high mechanical strength (69-156 MPa), high elastic modulus (152-173 GPa), low absorptivity (0.01-0.02 wt.%) and low thermal expansion coefficient (room temperature-600 °C, 0.9-1.6 × 10 -6 ℃ -1 ), which can meet the performance requirements of high-performance cordierite ceramic materials for high-precision equipment such as lithography machine mobile platforms. DETAILED DESCRIPTION

[0022] In order to further explain the present invention and the technical means and effects adopted to achieve the predetermined invention purpose, the present invention is described in detail below in conjunction with preferred embodiments: Example 1

[0023] Take 63 parts GeO 2 With 37 parts of SnO 2 Mix well, put into a corundum crucible, place in a high temperature electric furnace, heat to 1460℃ and keep warm for 2h, then quench with water, grind, dry and pass through a 250 sieve to obtain amorphous powder. Take 16 parts of magnesium oxide, 76 parts of kaolin (equivalent to 30 parts of Al 2 O 3 and 35.4 parts SiO 2 ) and 18.6 parts quartz, 1 part amorphous GeO 2 -SnO 2 micro powder, 53 parts of tap water, 0.7 parts of organic debonding agent, weigh and mix the raw materials evenly, then add 360 parts of ZrO 2The ball mill was used for ball milling for 3 hours. After the slurry was fully uniform, the slurry was poured out and passed through a 200-mesh standard sieve. The ceramic green body was obtained by slip casting. After drying at 70°C for 2 hours, it was heated to 1360°C at a heating rate of 5°C / min and kept warm for 2 hours. After cooling, a high elastic modulus dense cordierite ceramic material was obtained. Its flexural strength is 86MPa, elastic modulus is 152GPa, water absorption is 0.02wt%, and the average thermal expansion coefficient from room temperature to 600°C is 0.9×10 -6 ℃ -1 . Example 2

[0024] Take 56 parts of GeO 2 With 44 parts SnO 2 Mix well, put into a corundum crucible, place in a high temperature electric furnace, heat to 1510℃ and keep warm for 1.5h, quench with water, grind, dry and pass through 200 sieve to obtain amorphous powder. Take 15 parts of magnesium oxide, 83.5 parts of kaolin (equivalent to 33 parts of Al 2 O 3 and 39 parts SiO 2 ) and 13 parts quartz, 3 parts amorphous GeO 2 -SnO 2 powder, 51 parts of tap water, 0.6 parts of organic dissolving agent, weigh and mix the raw materials evenly, then add 350 parts of ZrO 2 The ball mill was used for ball milling for 2 hours. After the slurry was fully uniform, the slurry was poured out and passed through a 150-mesh standard sieve. The ceramic green body was obtained by slip casting. After drying at 60°C for 6 hours, it was heated to 1310°C at a heating rate of 20°C / min and kept warm for 2 hours. After cooling, a high elastic modulus dense cordierite ceramic material was obtained. Its flexural strength is 102MPa, elastic modulus is 165GPa, water absorption is 0.01wt%, and the average thermal expansion coefficient from room temperature to 600°C is 1.2×10 -6 ℃ -1 . Example 3

[0025] Take 78 parts GeO 2 With 22 parts SnO 2 Mix well, put into a quartz crucible, place in a high temperature electric furnace, heat to 1530℃ and keep warm for 3h, then quench with water, grind, dry and pass through a 300 sieve to obtain amorphous powder. Take 11 parts of magnesium oxide, 91 parts of kaolin (equivalent to 36 parts of Al 2 O 3 and 42.4 parts SiO 2 ) and 15.6 parts quartz, 6 parts amorphous GeO 2 -SnO 2powder, 60 parts of tap water, 0.8 parts of organic dissolving agent, weigh and mix the raw materials evenly, then add 380 parts of ZrO 2 The ball mill was used for ball milling for 2 hours. After the slurry was fully uniform, the slurry was poured out and passed through a 200-mesh standard sieve. The ceramic green body was obtained by slip casting. After drying at 80°C for 4 hours, it was heated to 1290°C at a heating rate of 3°C / min and kept warm for 1.5 hours. After cooling, a high elastic modulus dense cordierite ceramic material was obtained. Its flexural strength is 156MPa, elastic modulus is 173 GPa, water absorption is 0.01wt%, and the average thermal expansion coefficient from room temperature to 600°C is 1.6×10 -6 ℃ -1 .

Claims

1. A method for preparing a high elastic modulus dense cordierite ceramic material, characterized in that The steps include: Step 1: Preparation of GeO2-SnO2 system amorphous additive; Step 2: Prepare a cordierite ceramic raw material according to the weight percentage of MgO 11-16%, Al2O3 29-37%, and SiO2 51-59%, and then add the amorphous additive obtained in step 1, tap water, and an organic debonding agent, and obtain a high elastic modulus and dense cordierite ceramic material after weighing, mixing, ball milling, sieving, slip casting, green body drying, high temperature firing, and cooling; The preparation steps of the GeO2-SnO2 system amorphous additive in step 1 are as follows: according to weight percentage: GeO2 55-78%, SnO2 22-45%, after the raw materials are evenly mixed, they are loaded into a corundum crucible or a quartz crucible, placed in a high-temperature electric furnace from room temperature to 1450-1550°C and kept warm for 1-3 hours to obtain a uniform melt, and the melt is water quenched, ball milled, dried, and passed through a 200-300 mesh standard sieve to obtain amorphous micropowder; In the step 2, the amount of the amorphous additive added is 1-6wt% of the weight of the cordierite ceramic raw material, the amount of tap water added is 30-35wt% of the total weight of the raw material and water, and the amount of the organic dissolving agent added is 0.3-0.5wt% of the total weight of the raw material and water; The high-performance cordierite ceramic material obtained in step 2 has a mechanical strength of 69-156 MPa, an elastic modulus of 152-173 GPa, a water absorption rate of 0.01-0.02 wt%, and a thermal expansion coefficient of 0.9-1.6×10 -6 ℃ -1 .

2. The preparation method according to claim 1, characterized in that: In the second step, MgO in the cordierite ceramic raw material is introduced as magnesium oxide, Al2O3 is introduced as kaolin, and SiO2 is introduced as kaolin and quartz.

3. The preparation method according to claim 2, characterized in that: The sum of the weight contents of K2O and Na2O in the kaolin is less than 0.1wt%, and the sum of the weights of Fe2O3 and TiO2 is less than 0.2wt%.

4. The preparation method according to claim 1, characterized in that: The ball mill used in the ball milling process of step 2 is ZrO2, and the added amount is 2 to 3 times the total mass of the raw materials and water; the ball milling time is 1 to 3 hours.

5. The preparation method according to claim 1, characterized in that: The mesh size of the sieve in the second step of the sieving process is 100-200 meshes; the temperature in the green body drying process is 60-80° C. and the drying time is 2-6 hours.

6. The preparation method according to claim 1, characterized in that: The system of the high temperature firing process in step 2 is to heat to 1290-1360° C. at a heating rate of 3-20° C. / min and keep the temperature for 1-3 hours.

7. The preparation method according to claim 1, characterized in that: The high-performance cordierite ceramic material obtained in step 2 can be applied to the mobile platform of a photolithography machine.