A catalyst for direct production of oxygenated substances by low-temperature oxidation of CH4 and coupling of CO2, and its preparation method and application
Through the preparation of X-Cu-ZSM-5 catalyst, the high energy consumption and complex process problems of low-temperature direct coupling reaction of CH4 and CO2 are solved, high-selective conversion at low temperature is achieved, the process is simplified and energy consumption is reduced.
Patent Information
- Application Number
- CN202211635986.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-20
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-12-20
AI Technical Summary
In the existing technology, the low-temperature direct coupling reaction of CH4 and CO2 has problems of high energy consumption and complex processes, and it is difficult to achieve effective conversion under low-temperature conditions, which limits its large-scale application.
X-Cu-ZSM-5 catalyst is used, in which Cu and Direct coupling reaction of CH4 and CO2 under low temperature conditions, applied in continuous trickle bed reactor.
It achieves highly selective conversion of CH4 and CO2 at low temperature, simplifies the catalyst preparation process, reduces energy consumption, and improves the feasibility of the reaction and product selectivity.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical engineering, and specifically relates to a catalyst for directly preparing oxides by low-temperature oxidation of CH4 and coupling of CO2, and a preparation method and application thereof. Background Art
[0002] Since the Industrial Revolution, CO2 emitted by the massive use of fossil energy has become the main factor causing global climate change and is primarily responsible for the global temperature rise! CH4 is the main component of natural gas, biogas, coalbed methane and shale gas. It is widely distributed in nature and is also a greenhouse gas, with a greenhouse effect that is about 20 times greater than that of CO2. Using CH4 to reform CO2 at high temperature to first convert it into CO and H2, and then hydrogenating CO to synthesize chemicals such as olefins, aromatics, methanol, and higher alcohols is currently the main way to solve the problem of excessive CH4 and CO2 emissions. However, the reforming reaction temperature is extremely high (above ~800°C), requiring a large amount of energy input, and its energy consumption accounts for more than 60% of the entire process. Therefore, the development of low-temperature direct coupling of CH4 and CO2 to synthesize high-value chemicals catalysts and industrially applicable process technologies has important theoretical and practical significance.
[0003] Chinese patent literature discloses a "method for the one-step conversion of CH4 and CO2 to acetic acid using low-temperature plasma and modified catalysts (molecular sieves, supported copper-based catalysts)" (publication numbers CN 111672543 A and CN 111675609 A). On the one hand, plasma itself is energy-intensive. On the other hand, the process has problems such as wide distribution of products, low selectivity for oxygen-containing compounds, and insufficient synthetic stability.
[0004] Chinese patent literature discloses "a copper-modified molecular sieve catalyst" (publication number CN112973784A), which is used to prepare methanol from methane, water vapor and oxygen. However, the preparation process of this catalyst is complicated and inevitably produces carbon dioxide.
[0005] Chinese patent literature discloses "a bimetallic high-efficiency catalyst for the co-conversion of CH4 and CO2 to produce ethanol / acetaldehyde" (publication number CN114029061A). The system used is photothermal synergistic catalysis, which is carried out in an intermittent reactor and has difficulties in application.
[0006] Chinese patent literature discloses "a catalyst and process for synthesizing acetic acid by step-wise conversion of CH4-CO2" (publication numbers CN101357313A, CN1634841A, CN1309114A), which mainly utilizes separate feeding of CH4 and CO2, and utilizes overflow and replenishment of H2 to overcome thermodynamic barriers. This system also has the problem of complex process.
[0007] At present, as the environmental problems caused by CO2 have received increasing attention, the direct conversion of CH4 and CO2 to produce oxygen-containing compounds by catalytic methods has received great attention in the literature. However, most studies focus on DFT calculations, solid-state NMR, and in situ infrared characterization (J. Am. Chem. Soc., 2016, 138, 10191-10198; J. Phys. Chem. C., 2018, 122,9570-9577; ACS Catal., 2017, 7, 6719−6728; Chem. Commun., 2020, 56, 3983-3986), and there are few reports on experimental research.
[0008] In summary, at present, CH4 and CO2 are difficult to activate due to the stability of their own structures, which limits their large-scale application. Therefore, it is urgent to develop new catalytic systems and new processes. Summary of the invention
[0009] The main purpose of the present invention is to overcome the deficiencies in the prior art, solve the problems of high energy consumption CH4-CO2 reforming technology and mismatch of multi-step reaction process conditions in the prior art, as well as the problem that the reaction under low temperature conditions is subject to dual kinetic and thermodynamic limitations, resulting in difficulty in carrying out the reaction, and provide a catalyst for low-temperature oxidation of CH4 coupling CO2 to directly produce oxides, which is feasible at low temperature and has a simple preparation process, as well as a preparation method and application thereof.
[0010] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0011] A catalyst for directly preparing oxides by low-temperature oxidation of CH4 and coupling of CO2, wherein: the catalyst is in the form of X-Cu-ZSM-5, wherein ZSM-5 is a carrier, Cu and X are active components, and X is at least two of alkali metals, Zn, Ce, In, Co, Fe, Pd or Rh.
[0012] Furthermore, the mass fractions of Cu and X in the catalyst are both ≤5%, and the molar ratio of Cu:X is (10:1) to (1:10); the carrier is H-ZSM-5 molecular sieve, and the mass percentages of Si element and Al element in the molecular sieve are 15 wt. %~100 wt. %.
[0013] A method for preparing the above catalyst comprises the following steps:
[0014] S1. First ion exchange: add the first metal salt of X into deionized water to prepare a mixed solution with a concentration of 0.01-1 mol / L, then add H-ZSM-5 molecular sieve into the mixed solution to prepare a suspension, stir at a water bath temperature of 50°C-80°C for 6 h-12 h, and after the first ion exchange is completed, filter, wash, dry and calcine in sequence to obtain an ion-exchanged ZSM-5 solid powder;
[0015] S2, second ion exchange: add the second metal salt of X into deionized water to prepare a solution with a concentration of 0.05-0.5 mol / L, then add the ion-exchanged ZSM-5 solid powder prepared in step S1 into the mixed solution to prepare a suspension, stir at a water bath temperature of 50°C-80°C for 6 h-12 h, and after the second ion exchange is completed, filter, wash, dry, roast, and granulate in sequence to obtain a catalyst powder, the particle size of the catalyst powder is 40 mesh-60 mesh;
[0016] S3. Catalyst reduction: placing the catalyst powder obtained in step S2 in a tubular heating furnace, purging it under an inert atmosphere for 0-1 h, then heating it from room temperature to 400°C-800°C under a mixed atmosphere of hydrogen and inert gas at a heating rate of 1-10°C / min, and reducing it for 3 h-8 h to obtain a finished catalyst.
[0017] Furthermore, the metal salt is nitrate, acetate or chloride.
[0018] Furthermore, in step S3, the volume fraction of H2 in the mixed atmosphere is 5% to 50%, and the inert gas in the mixed atmosphere is one or more of Ar, He or N2.
[0019] An application of the above catalyst: the catalyst is applied to a trickle bed reactor, the reaction pressure is normal pressure ~ 10MPa, the reaction temperature is room temperature ~ 100°C, GHSV = 1000 ~ 20000 h -1 , the CH4 / CO2 volume ratio is (10:1)-(1:10), the H2O2 solution flow rate is 0.01~1.0 mL / min, and the H2O2 concentration is 0.01~8 M.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The active components of the catalyst provided by the present invention are only metal Cu and X, and the preparation process is simple and has good reproducibility;
[0022] (2) When the catalyst provided by the present invention is applied to a continuous trickle bed reaction process, the reaction temperature is low (<100°C) and the selectivity of oxygen-containing compounds is high;
[0023] (3) Due to the presence of H2O2 solution, the present invention makes the thermodynamically unfavorable reaction of converting CH4-CO2 into oxygen-containing compounds feasible, making the conversion of two greenhouse gases, CH4-CO2, a practical process. DETAILED DESCRIPTION
[0024] The following specific examples are used to further describe in detail the catalyst for direct production of oxygenates by low-temperature oxidation of CH4 and coupling of CO2 provided by the present invention, as well as its preparation method and application. The described cases are part of the implementation cases of the present invention, not all implementation cases. The implementation cases in the present invention and other implementation cases obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.
[0025] Example 1
[0026] A method for preparing a catalyst for directly preparing an oxygenate by low-temperature oxidation of CH4 and coupling of CO2, comprising the following steps:
[0027] S1. First ion exchange: weigh 2.0 g of KNO3 and add it to 100 mL of deionized water, then add 4.0 g of H-ZSM-5 molecular sieve to make a suspension, where Si / Al=25 in the H-ZSM-5 molecular sieve; stir for 10 h in a water bath at 80°C, filter and wash three times after the first ion exchange, dry at 110°C for 12 h, grind and calcine at 550°C for 6 h to obtain a K ion-exchanged ZSM-5 solid powder;
[0028] S2, second ion exchange: weigh 12.1 g of Cu(NO3)2·3H2O and dissolve it in 100 mL of deionized water, then add the K ion-exchanged ZSM-5 solid powder prepared in step S1 to make a suspension, stir it in a water bath at 80°C for 10 h, filter, wash and dry it in turn after the second ion exchange, and calcine it at 550°C for 6 h to obtain K-Cu-ZSM-5 catalyst powder;
[0029] S3. Catalyst reduction: The K-Cu-ZSM-5 catalyst powder obtained in step S2 was placed in a tubular heating furnace, and reduced at 450°C for 3 h in a 10% H2-90% Ar atmosphere with a total flow rate of 100 mL / min to obtain a finished K-Cu-ZSM-5 catalyst.
[0030] The K-Cu-ZSM-5 catalyst product prepared in Example 1 was placed in a homemade continuous trickle bed for evaluation. The evaluation conditions were: CH4 / CO2 volume ratio of 1:1, H2O2 solution flow rate of 0.1 mL / min, concentration of 0.2 M, reaction temperature of 50°C, reaction pressure of 3 MPa, space velocity of 4800 h -1 , Results: Methanol yield 320 μmol / g cat / h, selectivity 100%.
[0031] Example 2
[0032] A method for preparing a catalyst for directly preparing an oxygenate by low-temperature oxidation of CH4 and coupling of CO2, comprising the following steps:
[0033] S1. First ion exchange: weigh 1.6 g of Fe(NO3)3·9H2O and add it to 150 mL of deionized water, then add 4.0 g of H-ZSM-5 molecular sieve to make a suspension, where Si / Al=30; stir for 5 h in a 70°C water bath. After the first ion exchange, filter and wash three times in sequence, dry at 100°C for 12 h, grind and calcine at 500°C for 6 h to obtain Fe ion-exchanged ZSM-5 solid powder;
[0034] S2, second ion exchange: weigh 12.1 g of Cu(NO3)2·3H2O and dissolve it in 100 mL of deionized water, then add the Fe ion-exchanged ZSM-5 solid powder prepared in step S1 to make a suspension, stir it in a water bath at 80°C for 10 h, filter, wash and dry it in turn after the second ion exchange, and calcine it at 450°C for 6 h to obtain Fe-Cu-ZSM-5 catalyst powder;
[0035] S3. Catalyst reduction: The Fe-Cu-ZSM-5 catalyst powder obtained in step S2 was placed in a tubular heating furnace and reduced at 450°C for 5 h in a 50% H2-50% Ar atmosphere with a total flow rate of 100 mL / min to obtain a finished Fe-Cu-ZSM-5 catalyst.
[0036] The Fe-Cu-ZSM-5 catalyst product prepared in Example 2 was placed in a homemade continuous trickle bed for evaluation. The evaluation conditions were: CH4 / CO2 volume ratio of 2:1, H2O2 solution flow rate of 0.2 mL / min, concentration of 0.2 M, reaction temperature of 75°C, reaction pressure of 4 MPa, space velocity of 1000 h -1 , Results: Methanol yield 105 μmol / g cat / h, selectivity 36.8%, acetic acid yield 180 μmol / gcat / h, selectivity 63.2%.
[0037] Example 3
[0038] A method for preparing a catalyst for directly preparing an oxygenate by low-temperature oxidation of CH4 and coupling of CO2, comprising the following steps:
[0039] S1. First ion exchange: weigh 0.89 g of Zn(NO3)2·6H2O and add it to 200 mL of deionized water, then add 4.0 g of H-ZSM-5 molecular sieve to make a suspension, where Si / Al=38 in the H-ZSM-5 molecular sieve; stir for 5 h in a 70°C water bath, filter and wash three times after the first ion exchange, dry at 100°C for 12 h, grind and calcine at 450°C for 6 h to obtain Zn ion-exchanged ZSM-5 solid powder;
[0040] S2, second ion exchange: weigh 8.2 g of Cu(NO3)2·3H2O and dissolve it in 100 mL of deionized water, then add the Zn ion-exchanged ZSM-5 solid powder prepared in step S1 to make a suspension, stir it in a water bath at 80°C for 10 h, filter, wash, dry at 100°C, and calcine at 500°C for 6 h after the second ion exchange is completed, and obtain Zn-Cu-ZSM-5 catalyst powder;
[0041] S3. Catalyst reduction: The Zn-Cu-ZSM-5 catalyst powder obtained in step S2 is placed in a tubular heating furnace, and reduced at 400°C for 6 h in a 10% H2-90% He atmosphere with a total flow rate of 100 mL / min to obtain a Zn-Cu-ZSM-5 catalyst product.
[0042] The finished Zn-Cu-ZSM-5 catalyst prepared in Example 3 was placed in a homemade continuous trickle bed for evaluation. The evaluation conditions were: CH4 / CO2 volume ratio of 10:1, H2O2 solution flow rate of 1.0 mL / min, concentration of 5.0 M, reaction temperature of 25°C, reaction pressure of 5 MPa, space velocity of 10000 h -1 , Results: Methanol yield 220 μmol / g cat / h, selectivity 78.6%, acetic acid yield 60 μmol / g cat / h, selectivity 21.4%.
[0043] Example 4
[0044] A method for preparing a catalyst for directly preparing an oxygenate by low-temperature oxidation of CH4 and coupling of CO2, comprising the following steps:
[0045] S1. First ion exchange: weigh 1.7275 g of cobalt acetate and add it to 100 mL of deionized water, then add 4.0 g of H-ZSM-5 molecular sieve to prepare a suspension, wherein Si / Al in the H-ZSM-5 molecular sieve is 25; stir for 20 h in a 50°C water bath, filter and wash three times after the first ion exchange, dry at 110°C for 12 h, grind and calcine at 550°C for 6 h to obtain Co ion-exchanged ZSM-5 solid powder;
[0046] S2, second ion exchange: weigh 2.3 g of Cu(NO3)2·3H2O and dissolve it in 100 mL of deionized water, then add the Co ion-exchanged ZSM-5 solid powder prepared in step S1 to make a suspension, stir it in a water bath at 80°C for 10 h, filter, wash and dry it in turn after the second ion exchange, and calcine it at 550°C for 6 h to obtain Co-Cu-ZSM-5 catalyst powder;
[0047] S3. Catalyst reduction: The Co-Cu-ZSM-5 catalyst powder obtained in step S2 was placed in a tubular heating furnace and reduced at 450°C for 5h in a 40%H2-60%rN2 atmosphere with a total flow rate of 100 mL / min to obtain a Co-Cu-ZSM-5 catalyst product.
[0048] The Co-Cu-ZSM-5 catalyst product prepared in Example 4 was placed in a homemade continuous trickle bed for evaluation. The evaluation conditions were: CH4 / CO2 volume ratio of 8:1, H2O2 solution flow rate of 0.25 mL / min, concentration of 3.0 M, reaction temperature of 50°C, reaction pressure of 3 MPa, space velocity of 3000 h -1 , Results: Methanol yield 105 μmol / g cat / h, selectivity 29.6%, acetic acid yield 250 μmol / g cat / h, selectivity 70.4%.
[0049] Example 5
[0050] A method for preparing a catalyst for directly preparing an oxygenate by low-temperature oxidation of CH4 and coupling of CO2, comprising the following steps:
[0051] S1. First ion exchange: weigh 1.4 g of palladium chloride and add it to 150 mL of deionized water, then add 4.0 g of H-ZSM-5 molecular sieve to make a suspension, where Si / Al=15 in the H-ZSM-5 molecular sieve; stir for 12 h in a 30°C water bath, filter and wash three times after the first ion exchange, dry at 100°C for 12 h, grind and calcine at 500°C for 4 h to obtain a Pd ion-exchanged ZSM-5 solid powder;
[0052] S2, second ion exchange: weigh 3.5 g of Cu(NO3)2·3H2O and dissolve it in 100 mL of deionized water, then add the Pd ion-exchanged ZSM-5 solid powder prepared in step S1 to make a suspension, stir it in a water bath at 30°C for 10 h, filter, wash and dry it in turn after the second ion exchange, and calcine it at 450°C for 6 h to obtain Pd-Cu-ZSM-5 catalyst powder;
[0053] S3. Catalyst reduction: The Pd-Cu-ZSM-5 catalyst powder obtained in step S2 was placed in a tubular heating furnace, and reduced at 450°C for 5 h in a 20% H2-80% Ar atmosphere with a total flow rate of 100 mL / min to obtain a finished Pd-Cu-ZSM-5 catalyst.
[0054] The Pd-Cu-ZSM-5 catalyst product prepared in Example 5 was placed in a homemade continuous trickle bed for evaluation. The evaluation conditions were: CH4 / CO2 volume ratio of 1:3, H2O2 solution flow rate of 0.25 mL / min, concentration of 2.0 M, reaction temperature of 50°C, reaction pressure of 3.0 MPa, space velocity of 5000 h -1 , Results: Methanol yield 52 μmol / g cat / h, selectivity 13.4%, acetic acid yield 336 μmol / g cat / h, selectivity 86.6%.
[0055] Example 6
[0056] A method for preparing a catalyst for directly preparing an oxygenate by low-temperature oxidation of CH4 and coupling of CO2, comprising the following steps:
[0057] S1. First ion exchange: weigh 1.1 g of rhodium chloride and add it to 200 mL of deionized water, then add 4.0 g of H-ZSM-5 molecular sieve to make a suspension, where Si / Al=25 in the H-ZSM-5 molecular sieve; stir for 6 h in a water bath at 80°C, filter and wash three times after the first ion exchange, dry at 120°C for 12 h, grind and calcine at 400°C for 2 h to obtain Rh ion-exchanged ZSM-5 solid powder;
[0058] S2, second ion exchange: weigh 3.5 g of Cu(NO3)2·3H2O and dissolve it in 100 mL of deionized water, then add the Rh ion-exchanged ZSM-5 solid powder prepared in step S1 to make a suspension, stir it in a water bath at 80°C for 6 hours, and after the second ion exchange is completed, filter, wash, dry at 100°C, and calcine at 400°C for 3 hours to obtain Rh-Cu-ZSM-5 catalyst powder;
[0059] S3. Catalyst reduction: The Rh-Cu-ZSM-5 catalyst powder obtained in step S2 was placed in a tubular heating furnace and reduced at 400°C for 3h in a 30%H2-70%N2 atmosphere with a total flow rate of 100 mL / min to obtain a finished Rh-Cu-ZSM-5 catalyst.
[0060] The Rh-Cu-ZSM-5 catalyst product prepared in Example 6 was placed in a homemade continuous trickle bed for evaluation. The evaluation conditions were: CH4 / CO2 volume ratio of 1:5, H2O2 solution flow rate of 0.3 mL / min, concentration of 4.0 M, reaction temperature of 50°C, reaction pressure of 1.0 MPa, space velocity of 10000 h -1 , Results: Methanol yield 96 μmol / g cat / h, selectivity 27.4%, acetic acid yield 254 μmol / g cat / h, selectivity 72.6%.
[0061] Example 7
[0062] A method for preparing a catalyst for directly preparing an oxygenate by low-temperature oxidation of CH4 and coupling of CO2, comprising the following steps:
[0063] S1. First ion exchange: weigh 2.8 g of indium nitrate and add it to 100 mL of deionized water, then add 4.0 g of H-ZSM-5 molecular sieve to prepare a suspension, wherein Si / Al in the H-ZSM-5 molecular sieve is 100; stir for 6 h in a water bath at 80 °C, filter and wash three times after the first ion exchange, dry at 100 °C for 12 h, grind and calcine at 500 °C for 3 h to obtain In ion-exchanged ZSM-5 solid powder;
[0064] S2, second ion exchange: weigh 6.5 g of Cu(NO3)2·3H2O and dissolve it in 100 mL of deionized water, then add the In ion-exchanged ZSM-5 solid powder prepared in step S1 to make a suspension, stir it in a water bath at 80°C for 6 hours, and after the second ion exchange is completed, filter, wash, dry at 100°C, and calcine at 400°C for 5 hours to obtain In-Cu-ZSM-5 catalyst powder;
[0065] S3. Catalyst reduction: The In-Cu-ZSM-5 catalyst powder obtained in step S2 was placed in a tubular heating furnace and reduced at 400°C for 3h in a 10%H2-90%Ar atmosphere with a total flow rate of 100 mL / min to obtain a finished In-Cu-ZSM-5 catalyst.
[0066] The In-Cu-ZSM-5 catalyst product prepared in Example 7 was placed in a homemade continuous trickle bed for evaluation. The evaluation conditions were: CH4 / CO2 volume ratio of 1:2, H2O2 solution flow rate of 0.1 mL / min, concentration of 0.5 M, reaction temperature of 75°C, reaction pressure of normal pressure, space velocity of 5000 h -1 , Results: Methanol yield 220 μmol / g cat / h, selectivity 72.1%, acetic acid yield 85 μmol / g cat / h, selectivity 27.9%.
[0067] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A catalyst for the low temperature oxidation of CH 4 Coupling CO 2 Application in direct preparation of oxygenates, Features: The catalyst is applied to a trickle bed reactor, the reaction pressure is normal pressure to 10 MPa, the reaction temperature is room temperature to 100°C, and the GHSV is 1000 to 20000 h -1 , CH 4 / CO 2 The volume ratio is (10:1)-(1:10), H 2 O 2 The solution flow rate is 0.01~1.0 mL / min, H 2 O 2 Concentration ranges from 0.01 to 8 M; The oxygenate includes one or more of methanol and acetic acid; The catalyst is in the form of X-Cu-ZSM-5, wherein ZSM-5 is a carrier, Cu and X are active components, the mass fractions of Cu and X are both ≤5%, and the molar ratio of Cu:X is (10:1) to (1:10); X is one of alkali metals, Zn, Ce, In, Co, Fe, Pd or Rh.
2. The use according to claim 1, Features: The carrier is H-ZSM-5 molecular sieve, and the mass percentage of Si and Al in the molecular sieve is 15 wt .%~100 wt .%.
3. The use according to claim 2, It is characterized in that The preparation method of the catalyst comprises the following steps: S1. First ion exchange: Add the metal salt of X into deionized water to prepare a mixed solution with a concentration of 0.01-1 mol / L, then add H-ZSM-5 molecular sieve into the mixed solution to prepare a suspension, stir at a water bath temperature of 50°C-80°C for 6 h-12 h, and after the first ion exchange is completed, filter, wash, dry and calcine in sequence to obtain an ion-exchanged ZSM-5 solid powder; S2, second ion exchange: adding Cu metal salt to deionized water to prepare a solution with a concentration of 0.05-0.5 mol / L, then adding the ion-exchanged ZSM-5 solid powder prepared in step S1 to the solution to prepare a suspension, stirring at a water bath temperature of 50°C-80°C for 6 h-12 h, and filtering, washing, drying, calcining, and granulating in sequence after the second ion exchange to obtain a catalyst powder with a particle size of 40-60 mesh; S3. Catalyst reduction: placing the catalyst powder obtained in step S2 in a tubular heating furnace, purging it under an inert atmosphere for 0-1 h, then heating it from room temperature to 400°C-800°C in a mixed atmosphere of hydrogen and inert gas at a heating rate of 1-10°C / min, and reducing it for 3 h-8 h to obtain a finished catalyst.
4. The use according to claim 3, Features: The metal salt of X is nitrate, acetate or chloride.
5. The use according to claim 3, Features: In step S3, H 2 The volume fraction is 5%~50%, and the inert gas in the mixed atmosphere is Ar, He or N 2 One or more of.