A titanium silicon molecular sieve and its synthesis method and application

By using tetramethoxysilane and tetrabutyl titanate to synthesize titanium-silicon molecular sieves, the problem of high synthesis cost of titanium-silicon molecular sieves is solved, and the same catalytic performance as high-performance titanium-silicon molecular sieves is achieved. Application in chemical reactions reduces costs and maintains high efficiency.

CN115974094BActive Publication Date: 2024-10-01CHINA CATALYST HLDG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211655532.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-10-01
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The synthesis cost of existing titanium-silicon molecular sieves is high, and the method using ethyl orthosilicate as the silicon source has better catalytic performance, but it is expensive. How to reduce the synthesis cost while ensuring the catalytic performance.

Method used

Using tetramethoxysilane as the silicon source, tetrabutyl titanate as the titanium source, and tetrapropylammonium hydroxide as the template agent, titanium-silicon molecular sieves were synthesized through a hydrothermal method. The synthesis conditions were controlled to reduce costs, and in the allyl group This catalyst is used in chlorine epoxidation reactions.

Benefits of technology

It significantly reduces the synthesis cost of titanium-silicon molecular sieves, and at the same time maintains the same catalytic performance as that synthesized using ethyl orthosilicate as raw material in the allyl chloride epoxidation reaction, and has industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004010921380000011
    Figure HDA0004010921380000011
  • Figure HDA0004010921380000012
    Figure HDA0004010921380000012
  • Figure HDA0004010921380000013
    Figure HDA0004010921380000013
Patent Text Reader

Abstract

The present invention discloses a titanium silicon molecular sieve and its synthesis method and application. The titanium silicon molecular sieve is synthesized by a hydrothermal method using tetramethoxysilane as a silicon source, tetrabutyl titanate as a titanium source, tetrapropylammonium hydroxide as a template, ethanol and isopropanol as solvents. The present invention uses tetramethoxysilane to replace the tetraethyl orthosilicate in the traditional hydrothermal method, and the catalytic performance of the titanium silicon molecular sieve synthesized with tetraethyl orthosilicate as a raw material can still be achieved. However, since the market price of tetramethoxysilane is much lower than that of tetraethyl orthosilicate, this significantly reduces the production cost of the titanium silicon molecular sieve, so the synthesis of the titanium silicon molecular sieve using tetramethoxysilane as a raw material has industrial significance for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of molecular sieve material preparation, and relates to a method for synthesizing titanium silicon molecular sieve by taking tetramethoxysilane as raw material and application of the method in allyl chloride epoxidation reaction. Background Art

[0002] Titanium silicate molecular sieve TS-1 belongs to the orthorhombic system and has the same MFI topological structure as ZSM-5 molecular sieve. Due to the introduction of transition metal titanium, TS-1 has unique catalytic oxidation performance. TS-1 is widely used in catalytic oxidation reactions such as olefin epoxidation, hydroxylation of phenol and benzene, partial oxidation of alkanes, oxidation of alcohols, and oximation of ketones.

[0003] Titanium silicate molecular sieve is usually synthesized by hydrothermal method. At present, the synthesis system is mainly divided into two categories, one is the synthesis system with tetraethyl orthosilicate as silicon source and tetrapropylammonium hydroxide as template, and the other is the synthesis system with silica sol as silicon source and tetrapropylammonium bromide as template. The former has a high synthesis cost due to the high price of tetraethyl orthosilicate and tetrapropylammonium hydroxide, while the latter has a lower cost but poorer catalytic performance than the former. Therefore, how to reduce the synthesis cost of titanium silicate molecular sieve while ensuring better catalytic performance is of practical and industrial production significance.

[0004] Patent CN107500309B discloses a method for preparing titanium silicon molecular sieve, using tetraethyl orthosilicate as silicon source and tetrabutyl titanate as titanium source. The molecular sieve preparation process includes hydrolysis of silicon source and titanium source, dealcoholization, crystallization, filtration, roasting, modification and other steps. The final catalyst is used for and undergoes two dealcoholizations. After the silicon source is hydrolyzed, the titanium source is hydrolyzed. Cyclohexanone ammoxidation is performed to prepare cyclohexanone oxime.

[0005] Patent CN103641134B describes a method for preparing a titanium silicon molecular sieve with controllable grain size. Ethyl orthosilicate, tetrabutyl titanate, a template, an alkali source, an inorganic ammonium salt and a molecular sieve mother liquor are mixed in a molar ratio of SiO2:TiO2:template:alkali source:inorganic ammonium salt:H2O of 1:0.01-0.04:0.2-0.6:0.1-3.0:0-0.3:20-60, and crystallization is performed. The titanium silicon molecular sieve synthesized by this method has a small grain size, high crystallinity, high skeleton titanium content, strong hydrophobicity, and has high activity for selective oxidation reactions such as olefin epoxidation, aromatic hydrocarbon hydroxylation, and ketone ammoxidation.

[0006] Patent CN103214000B discloses a method for synthesizing titanium silicon molecular sieve TS-1, wherein the silicon source is first subjected to acid-catalyzed hydrolysis, and then the titanium source is simultaneously subjected to base-catalyzed hydrolysis, and the silicon source can be selected from one or a mixture of two or more of methyl orthosilicate, ethyl orthosilicate, and butyl orthosilicate. However, the specific process and application of synthesizing titanium silicon molecular sieve using methyl orthosilicate as a silicon source are not specifically described in the specific embodiments.

[0007] It can be seen that the synthesis of titanium silicon molecular sieve using tetramethoxysilane as a silicon source is not a conventional technical means. This may be due to the difference in the hydrolysis rate of tetramethoxysilane and ethyl orthosilicate. The hydrolysis rate of the former is very fast and difficult to control. However, compared with the prices of the two, the price of tetramethoxysilane is only about one-third of the price of ethyl orthosilicate, and to obtain the same silicon content, the amount of tetramethoxysilane used is three-quarters of the amount of ethyl orthosilicate used. Therefore, if tetramethoxysilane is used as a raw material to synthesize titanium silicon molecular sieve, the synthesis cost of molecular sieve can be greatly reduced. Summary of the invention

[0008] The invention provides a method for synthesizing titanium silicalite by using tetramethoxysilane as a raw material. The synthesized TS-1 has the same catalytic performance as TS-1 synthesized by using ethyl orthosilicate as a raw material. The method significantly reduces the synthesis cost of the titanium silicalite and has industrial significance.

[0009] In order to achieve the above purpose and effect, the following scheme is adopted:

[0010] A method for synthesizing titanium silicon molecular sieve, using tetramethoxysilane as a silicon source, tetrabutyl titanate as a titanium source, tetrapropylammonium hydroxide as a template, ethanol and isopropanol as solvents, and hydrothermal method to synthesize titanium silicon molecular sieve. The specific synthesis steps are as follows:

[0011] (1) Tetramethoxysilane and ethanol are mixed, stirred and heated to 50-80°C, tetrabutyl titanate is added dropwise, the mixture is stirred and kept warm for 1-5 hours, and then the temperature is lowered to 20-30°C.

[0012] (2) Add tetrapropylammonium hydroxide aqueous solution dropwise to the mixture in (1), control the temperature in the autoclave to be below 40°C, and stir for 2 to 4 hours after the addition is complete.

[0013] (3) Mix tetrabutyl titanate and isopropanol and add dropwise to the mixture in (2), control the temperature in the autoclave to be below 40° C., and stir for 1 to 2 hours after the addition is complete.

[0014] (4) The mixture in (3) is heated to dealcoholize and add water, wherein the dealcoholization temperature is 80-90° C., the dealcoholization amount is 60-80% of the total feed amount, and the water addition amount is 30-50% of the total feed amount.

[0015] (5) The mixture in (4) is placed in a stainless steel high-pressure reactor, crystallized at 160-180° C. for 48-120 h, cooled, filtered, washed, dried at 80-100° C., and calcined at 500-600° C. to obtain a titanium silicon molecular sieve.

[0016] Furthermore, in the synthesis method described above, the mass ratio of the feed amounts of the various materials is tetramethoxysilane: ethanol: tetrabutyl titanate: isopropanol: tetrapropylammonium hydroxide: water = 1: 0.6-1.5: 0.06-0.08: 0.3-0.7: 0.2-0.5: 1-2.

[0017] Furthermore, in the above-mentioned synthesis method, the amount of tetrabutyl titanate added in step (1) is 0.1 to 1.5% of the weight of tetramethoxysilane.

[0018] The present invention provides a titanium silicon molecular sieve synthesized by the method.

[0019] The present invention provides application of the titanium silicon molecular sieve in the epoxidation reaction of allyl chloride.

[0020] Furthermore, in the above technical solution, in the epoxidation reaction of allyl chloride, the molar ratio of allyl chloride to H2O2 is 2 to 5:1, and the mass ratio of methanol to hydrogen peroxide is 4 to 10:1.

[0021] Furthermore, in the above technical solution, in the epoxidation reaction of allyl chloride, the reaction temperature is 30-45°C, the reaction pressure is 0.2-1.0 MPa, and the mass space velocity of allyl chloride is 0.5-5 h -1 .

[0022] The present invention is further described below with specific examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD spectrum of titanium silicalite C-1;

[0024] Figure 2 This is the SEM photo of titanium silicate molecular sieve C-1;

[0025] Figure 3 This is the XRD spectrum of titanium silicalite D-1;

[0026] Figure 4 This is the SEM photo of titanium silicate molecular sieve D-1;

[0027] Figure 5 This is the SEM photo of titanium silicate molecular sieve D-2. DETAILED DESCRIPTION

[0028] The present invention is further described in the following examples, but the present invention is not limited thereto.

[0029] The purity of the materials used in the examples is not less than 99%.

[0030] The titanium silicalite synthesized by the present invention is used in the fixed bed reaction of allyl chloride epoxidation. Inert quartz sand is added to both ends of the stainless steel jacket reaction tube, and 6g of titanium silicalite (20-40 mesh) is filled in the middle. The temperature of the reactor is maintained by a super constant temperature water bath. The reactants hydrogen peroxide, allyl chloride and solvent methanol are fed simultaneously. The product analysis is carried out regularly. The reaction index is the H2O2 conversion rate (X H2O2 ) and the selectivity of epoxidation products (S ECH ). The reaction index is calculated as follows:

[0031] H2O2 conversion rate X = number of moles of H2O2 reacted / total number of moles of H2O2 * 100%;

[0032] Epichlorohydrin Selective S ECH = Number of moles of epichlorohydrin produced by the reaction / number of moles of H2O2 reacted * 100%.

[0033] The XRD characterization of the catalyst was measured by X-ray diffraction analyzer (PANalytical, X'Pert3 Powder).

[0034] The catalyst scanning electron microscopy (SEM) characterization was measured by scanning electron microscope (Hitachi, SU5000).

[0035] Example 1

[0036] Mix 500g of tetramethoxysilane with 453g of ethanol, stir and heat to 60℃, add 2.5g of tetrabutyl titanate, keep warm and stir for 3h, then cool to 30℃. Add 750g of 18% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition is complete. Mix 32.5g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is complete. Heat up, dealcoholate, dealcoholate temperature 80-90℃, dealcoholate amount 1350g, make up 897g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, calcined at 500℃ for 6h, and titanium silicon molecular sieve is obtained, recorded as C-1.

[0037] The XRD spectrum and SEM photos of titanium silicate molecular sieve C-1 are attached. Figure 1 and attached Figure 2 .

[0038] Example 2

[0039] Mix 500g of tetramethoxysilane with 302g of ethanol, stir and heat to 60℃, add 2.5g of tetrabutyl titanate, keep warm and stir for 3h, then cool to 30℃. Add 750g of 18% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition is complete. Mix 32.5g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is complete. Heat up, dealcoholate, dealcoholate temperature 80-90℃, dealcoholate amount 1202g, add 900g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, calcined at 500℃ for 6h, and titanium silicon molecular sieve is obtained, recorded as C-2.

[0040] Example 3

[0041] Mix 500g of tetramethoxysilane with 605g of ethanol, stir and heat to 60℃, add 2.5g of tetrabutyl titanate, keep warm and stir for 3h, then cool to 30℃. Add 750g of 18% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition. Mix 32.5g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition. Heat up, dealcoholization, dealcoholization temperature 80-90℃, dealcoholization amount 1500g, and make up 895g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, and calcined at 500℃ for 6h to obtain titanium silicon molecular sieve, recorded as C-3.

[0042] Example 4

[0043] Mix 500g of tetramethoxysilane with 453g of ethanol, stir and heat to 60℃, add 1g of tetrabutyl titanate, keep warm and stir for 5h, then cool to 30℃. Add 750g of 18% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition is complete. Mix 34g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is complete. Heat up, dealcoholization, dealcoholization temperature 80-90℃, dealcoholization amount 1350g, make up 897g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, calcined at 500℃ for 6h, and titanium silicon molecular sieve is obtained, recorded as C-4.

[0044] Example 5

[0045] Mix 500g of tetramethoxysilane with 453g of ethanol, stir and heat to 60℃, add 5g of tetrabutyl titanate, keep warm and stir for 1h, then cool to 30℃. Add 750g of 18% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition is complete. Mix 30g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is complete. Heat up, dealcoholization, dealcoholization temperature 80-90℃, dealcoholization amount 1350g, make up 897g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, calcined at 500℃ for 6h, and titanium silicon molecular sieve is obtained, recorded as C-5.

[0046] Example 6

[0047] Mix 500g of tetramethoxysilane with 453g of ethanol, stir and heat to 80℃, add 2.5g of tetrabutyl titanate, keep warm and stir for 3h, then cool to 30℃. Add 750g of 18% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition is complete. Mix 32.5g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is complete. Heat up, dealcoholization, dealcoholization temperature 80-90℃, dealcoholization amount 1350g, make up 897g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, calcined at 500℃ for 6h, and titanium silicon molecular sieve is obtained, recorded as C-6.

[0048] Example 7

[0049] Mix 500g of tetramethoxysilane with 453g of ethanol, stir and heat to 60℃, add 2.5g of tetrabutyl titanate, keep warm and stir for 3h, then cool to 30℃. Add 925g of 19% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition is complete. Mix 37.5g of tetrabutyl titanate with 300g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is complete. Heat up, dealcoholization, dealcoholization temperature 80-90℃, dealcoholization amount 1400g, and make up 947g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, and calcined at 500℃ for 6h to obtain titanium silicon molecular sieve, recorded as C-7.

[0050] Example 8

[0051] Mix 500g of tetramethoxysilane with 453g of ethanol, stir and heat to 60℃, add 2.5g of tetrabutyl titanate, keep warm and stir for 3h, then cool to 30℃. Add 610g of 18% tetrapropylammonium hydroxide aqueous solution, control the temperature in the kettle below 40℃, and stir for 3h after the addition is complete. Mix 27.5g of tetrabutyl titanate with 200g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is complete. Heat up, dealcoholization, dealcoholization temperature 80-90℃, dealcoholization amount 1300g, make up 847g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, calcined at 500℃ for 6h, and titanium silicon molecular sieve is obtained, recorded as C-8.

[0052] Comparative Example 1

[0053] Put 684g of tetraethyl orthosilicate into the kettle, add 750g of 18% tetrapropylammonium hydroxide aqueous solution at 30℃, control the temperature in the kettle below 40℃, and stir for 3h after the addition is completed. Mix 35g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is completed. Heat up, dealcoholate, the dealcoholate temperature is 80-90℃, the dealcoholate amount is 900g, and water is added 900g. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, and roasted at 500℃ for 6h to obtain titanium silicon molecular sieve, recorded as D-1.

[0054] The XRD spectrum and SEM photos of titanium silicate molecular sieve D-1 are attached. Figure 3 and attached Figure 4 .

[0055] Comparative Example 2

[0056] Put 500g of tetramethoxysilane into the kettle, add 750g of 18% tetrapropylammonium hydroxide aqueous solution at 30℃, control the temperature in the kettle below 40℃, and stir for 3h after the addition is completed. Mix 35g of tetrabutyl titanate with 250g of isopropanol, add the mixed materials to the kettle, control the temperature in the kettle below 40℃, and stir for 1h after the addition is completed. Heat up, dealcoholate, dealcoholate temperature 80-90℃, dealcoholate amount 1350g, make up 897g of water. The obtained material is loaded into a stainless steel high-pressure reactor, crystallized at 170℃ for 96h, cooled, filtered, washed to neutral, dried at 100℃, calcined at 500℃ for 6h, and titanium silicon molecular sieve is obtained, recorded as D-2.

[0057] See the attached SEM photo of titanium silicate molecular sieve D-2 Figure 5 .

[0058] Application Examples

[0059] The epoxidation performance of allyl chloride was evaluated for the catalyst samples obtained in the comparative example and the example. The epoxidation reaction was carried out in a fixed bed reactor, 6 g (20-40 mesh) of catalyst was loaded into the middle section of a stainless steel jacketed reaction tube, the upper and lower ends of the reaction tube were filled with inert quartz sand, the reaction pressure was 0.5 MPa, the reaction temperature was maintained at 40°C in a constant temperature water bath, the raw materials allyl chloride, hydrogen peroxide, and solvent methanol were fed simultaneously, and the allyl chloride space velocity was 2 h -1 The molar ratio of allyl chloride to H2O2 was 3, the mass ratio of methanol to hydrogen peroxide was 8, and samples were taken and analyzed after the reaction was carried out for 24 hours. The reaction results are shown in Table 1.

[0060] The performance evaluation results of the samples obtained in the comparative examples and embodiments are listed in Table 1.

[0061] It can be seen from the table below that the catalytic performance of the titanium silicate molecular sieve synthesized using tetramethoxysilane as raw material can reach the catalytic performance of the titanium silicate molecular sieve synthesized using ethyl orthosilicate as raw material.

[0062] Table 1 Catalytic performance evaluation results of each sample catalyst

[0063] Serial number catalyst <![CDATA[X H2O2 (%)]]> <![CDATA[S ECH (%)]]> Example 1 C-1 99.4 99.5 Example 2 C-2 99.6 99.0 Example 3 C-3 99.4 99.4 Example 4 C-4 99.5 99.3 Example 5 C-5 99.1 98.8 Example 6 C-6 99.2 99.2 Example 7 C-7 99.5 99.2 Example 8 C-8 99.0 99.4 Comparative Example 1 D-1 99.5 99.3 Comparative Example 2 D-2 97.5 97.3

Claims

1. A method for synthesizing titanium silicon molecular sieve, characterized in that: Titanium silicon molecular sieve was synthesized by hydrothermal method using tetramethoxysilane as silicon source, tetrabutyl titanate as titanium source, tetrapropylammonium hydroxide as template, ethanol and isopropanol as solvent. The specific synthesis steps are as follows: (1) Tetramethoxysilane and ethanol are mixed, stirred and heated to 50-80°C, tetrabutyl titanate is added dropwise, the mixture is stirred and kept warm for 1-5 hours, and then the temperature is lowered to 20-30°C; (2) adding an aqueous solution of tetrapropylammonium hydroxide to the mixture in (1), controlling the temperature in the kettle to be below 40° C., and stirring for 2 to 4 hours after the addition is complete; (3) tetrabutyl titanate and isopropyl alcohol are mixed and then added dropwise to the mixture in (2), the temperature in the autoclave is controlled to be lower than 40° C., and the mixture is stirred for 1 to 2 hours after the addition is completed; (4) heating the mixture in (3) to dealcoholize and add water, wherein the dealcoholization temperature is 80-90° C., the dealcoholization amount is 60-80% of the total feed amount, and the water addition amount is 30-50% of the total feed amount; (5) The mixture in (4) is placed in a stainless steel high-pressure reactor, crystallized at 160-180° C. for 48-120 h, cooled, filtered, washed, dried at 80-100° C., and calcined at 500-600° C. to obtain a titanium silicon molecular sieve.

2. The synthesis method according to claim 1, characterized in that The mass ratio of the feeding amount of each material is tetramethoxysilane: ethanol: tetrabutyl titanate: isopropanol: tetrapropylammonium hydroxide: water = 1: 0.6-1.5: 0.06-0.08: 0.3-0.7: 0.2-0.5: 1-2.

3. The synthesis method according to claim 1, characterized in that In step (1), the amount of tetrabutyl titanate added is 0.1 to 1.5% of the weight of tetramethoxysilane.

4. A titanium silicon molecular sieve synthesized by the method according to any one of claims 1 to 3.

5. Use of the titanium silicon molecular sieve according to claim 4 in the epoxidation reaction of allyl chloride.

6. The use according to claim 5, characterized in that: In the allyl chloride epoxidation reaction, the molar ratio of allyl chloride to H2O2 is 2-5:1, and the mass ratio of methanol to hydrogen peroxide is 4-10:

1.