A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve and preparation method thereof
Through the modified lithium titanium phosphate precursor modified by chromium ion and zirconium ion doping, a three-dimensional titanium phosphate framework co-top oxygen type lithium ion sieve was prepared, which solved the problem of low adsorption capacity and selectivity of the existing lithium ion sieve and achieved high efficiency , stable lithium ion adsorption and reusing performance, suitable for applications in lithium batteries and new energy fields.
Patent Information
- Application Number
- CN202211423165.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-15
AI Technical Summary
The adsorption capacity and selectivity of existing lithium-ion sieves are low, and the dissolution rate is high when reused, making it difficult to meet the high-efficiency lithium-enhancing needs of lithium-ion sieves in the fields of lithium batteries and new energy.
Using modified lithium titanium phosphate precursors doped with chromium ions and zirconium ions, a three-dimensional titanium phosphate skeleton co-top oxygen type lithium ion sieve is prepared through hydrothermal reaction, keeping the skeleton structure unchanged, improving ion exchange performance, improving adsorption capacity and selection sex.
It significantly improves the adsorption capacity and selectivity of lithium ions, enhances the stability and cyclicity of lithium ion sieve, reduces the titanium dissolution rate, and has a simple process and low cost, making it suitable for industrial production.
Smart Images

Figure CN115974099B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium salt extraction and separation, and relates to a lithium ion sieve, in particular to a three-dimensional titanium phosphate framework top oxygen-shared lithium ion sieve and a preparation method thereof. Background Art
[0002] With the rapid increase in industrial demand for lithium batteries and new lithium energy sources, the development and utilization of liquid lithium resources such as salt lake brine, seawater and geothermal water has gradually become a research hotspot. Ion sieve adsorption lithium extraction is an efficient and green lithium extraction method with large adsorption capacity, low cost and repeatability. In 1978, Arberti reported that polyvalent metal acid salts (such as zirconium phosphate) can also play the role of ion sieves. The interlayer spacing of polyvalent metal acid salts changes in the range of 0.7-1.2nm with changes in metal type and water content. Ions with large radius can be embedded in the polyvalent metal salts with large interlayer spacing. As the interlayer spacing decreases, ions with large radius gradually become difficult to embed.
[0003] Common lithium titanium phosphate is mostly used in battery materials, but due to its structural stability, lithium ions are difficult to desorb and it cannot be used as an ion sieve. Japanese scientist Yukako reported that lithium zirconium phosphate was doped with a small amount of chromium ions to form a zirconium chromium phosphate lithium precursor, which was obtained after acid washing. 2.5 Cr 1.5 Zr 0.5 (PO4)3, which has a high selectivity for sodium ions, an adsorption capacity of 96.485 mg / g, and a lithium ion adsorption capacity of 12.528 mg / g. (Journal of the Japan Seawater Society, 1992: 312-319). In 2002, Sun Zhengang et al. (CN1470477A) proposed a method for preparing trivalent metal zirconium phosphate inorganic material (MeZrPO-15), which can be used in ion exchange, adsorption, catalysis and other fields, but did not conduct performance research on the adsorption capacity and selectivity of lithium ion sieves. Regarding the selectivity of phosphate ion sieves, in 2018, Li Jiansheng et al. (CN108079936A) reported a phosphate-type lithium ion sieve filler and a preparation method thereof, which is a chromium phosphate lithium ion sieve filler loaded with a lightweight glass material coated with nano-titanium dioxide. Although a special coating method and carrier are used, the adsorption capacity of its lithium ion sieve filler is 15-20 mg / g, which is a low adsorption capacity.
[0004] The main technical parameters for evaluating ion sieves are adsorption capacity, adsorption selectivity, dissolution loss rate and repeatability. The present invention aims to seek a new type of lithium ion sieve with large adsorption capacity, high selectivity and small dissolution loss. Summary of the invention
[0005] The object of the present invention is to provide a lithium ion sieve, which is a new type of ternary metal lithium ion sieve with a three-dimensional titanium phosphate skeleton co-top oxygen structure, so as to achieve the effect of improving the adsorption capacity of the ion sieve, the selectivity and repeatability of lithium ions.
[0006] Another object of the present invention is to provide a method for preparing the lithium ion sieve.
[0007] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a three-dimensional titanium phosphate framework top oxygen-shared lithium ion sieve, which is a delithiation product of a modified lithium titanium phosphate precursor doped with chromium ions and zirconium ions, wherein the molecular formula of the modified lithium titanium phosphate is Li 1+x Ti y Cr x Zr 2-x-y (PO4)3 (denoted as L-TCZP), where x=0.1-1.4, y=0.4-0.6.
[0008] Preferably, the molecular formula of the modified lithium titanium phosphate is, wherein x=0.3-1.2, y=0.4-0.6; most preferably, x=0.5, y=0.5.
[0009] The lithium ion sieve of the present invention is Cr 3+ 、Zr 4+ Replace part of Ti 4+ Improve the ion exchange performance of LiTi2(PO4)3. LiTi2(PO4)3 is an ion conductor whose crystal structure is a three-dimensional [Ti2(PO4)3] composed of TiO6 octahedron and PO4 tetrahedron through shared apex oxygen. - The framework is modified by zirconium and chromium, and the framework structure remains unchanged. The ion sieve obtained after lithium removal has a three-dimensional [Ti2(PO4)3] composed of common apex oxygen. - framework, thereby improving the selectivity of the ion sieve and enhancing its stability and cyclability.
[0010] The lithium ion sieve is prepared by the following method:
[0011] A lithium source, a titanium source, a chromium source, a zirconium source and a phosphorus source are dissolved in a solvent and mixed, and the obtained mixed solution is subjected to a hydrothermal reaction, wherein the molar ratio of each metal ion in the titanium source, the chromium source, the zirconium source and the lithium source is Ti 4+ :Cr 3+ :Zr 4+ :Li + =y:x:(2-xy):(1+x), the molar ratio of titanium source to phosphorus source Ti 4+ :PO4 3- =y:3; After the hydrothermal reaction product is calcined, a modified lithium titanium phosphate precursor doped with chromium ions and zirconium ions is obtained, and the molecular formula is Li1+x Ti y Cr x Zr 2-x-y (PO4)3; the precursor is delithiated to obtain the lithium ion sieve, denoted as HTi y Cr x Zr 2-x-y (PO4)3, wherein x = 0.1-1.4, y = 0.4-0.6.
[0012] In the method described, the reaction principle of the precursor preparation is as follows:
[0013] Li + +Zr 4+ +Ti 4+ +Cr 3+ +PO4 3- →Li 1+x Ti y Cr x Zr 2-x-y (PO4)3
[0014] Precursor Li 1+x Ti y Cr x Zr 2-x-y (PO4)3(L-TCZP) compounds are prepared by conventional hydrothermal reactions, for example, by mixing Li2CO3, C 16 H 36 O4Ti, Zr(NO3)4·5H20, Cr(NO3)3·9H2O and (NH4)H2PO4 are dissolved in a solvent and mixed, the mixed solution is subjected to a hydrothermal reaction, the reaction product is dried, ground into powder particles and then calcined in a muffle furnace, and the calcined product is the ion sieve precursor.
[0015] Preferably, the titanium source is selected from inorganic or organic titanium such as tetrabutyl titanate, tetraisopropyl titanate, titanium acetate, titanium nitrate, titanium sulfate, titanium chloride, titanium dioxide, and titanic acid.
[0016] Preferably, the zirconium source is selected from soluble inorganic or organic zirconium salts such as zirconium nitrate, zirconium oxychloride, zirconium citrate, zirconium sulfate, zirconium propionate, or hydrates thereof.
[0017] Preferably, the chromium source is selected from soluble inorganic or organic chromium salts such as chromium nitrate, chromium hydrochloride, chromium sulfate, chromium carbonate, acetyl chromium, chromium nicotinate, etc.; or their hydrates.
[0018] Preferably, the lithium source is selected from lithium nitrate, lithium hydroxide or lithium carbonate.
[0019] Preferably, the phosphorus source is selected from phosphoric acid, hydrogen phosphate, dihydrogen phosphate or orthophosphate, preferably the sodium, potassium or ammonium salts thereof.
[0020] Furthermore, the solvent of the mixed solution is water, ethanol or a mixture of water and ethanol. Preferably, the solvent contains citric acid.
[0021] Preferably, the concentration of metal ions in the mixed solution is 0.1-10 mol / L.
[0022] Preferably, the temperature of the hydrothermal reaction is 120° C.-180° C., and the time of the hydrothermal reaction is 12-36 h.
[0023] Furthermore, the calcination temperature is 200-1200° C., preferably 300-1000° C.; and the calcination time is 6-24 hours.
[0024] Furthermore, the precursor is delithiated by acid leaching, and the acid used for the delithiation treatment of the doped lithium ion sieve precursor is preferably an acid solution such as hydrochloric acid, sulfuric acid, phosphoric acid, oxalic acid, nitric acid, formic acid, acetic acid, etc.
[0025] Preferably, the acid solution concentration for acid leaching lithium is 0.04-0.10 mol / L, and the immersion time is 24h-72h.
[0026] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0027] 1. The present invention adopts Cr and Zr dual ions as the metal cations for doping modification for the first time. Not only the valence state of zirconium ions is consistent with that of titanium ions, but also the radius of chromium ions and zirconium ions is very close to that of titanium ions. Doping will not cause the structure of the ion sieve to change, but will increase the elution rate of the precursor lithium ions. The adsorption performance of the ion sieve after doping becomes larger, and the cyclic adsorption performance is improved compared with the traditional titanium phosphate type lithium ion sieve. The modified ternary metal phosphate lithium ion sieve prepared by the hydrothermal method of the present invention has a three-dimensional [Ti2(PO4)3] structure composed of TiO6 octahedron and PO4 tetrahedron through shared apex oxygen. - Skeleton crystal structure.
[0028] 2. Compared with the traditional ion sieve, the doped modified ion sieve of the present invention has excellent structure and better particle morphology. Through electron microscopy comparison, the ion binding rate is also higher than that of single ion doping. The particle size is uniform, which is conducive to full contact with the solution during adsorption.
[0029] 3. The method of the present invention is simple to manufacture, low in cost, and easy to realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The precursor Li prepared in Example 1 of the present invention 1.5 Ti 0.5 Cr 0.5XRD pattern of Zr(PO4)3.
[0031] Figure 2 The ion sieve HTi prepared in Example 1 of the present invention 0.5 Cr 0.5 XRD pattern of Zr(PO4)3.
[0032] Figure 3 The precursor Li prepared in Example 1 of the present invention 1.5 Ti 0.5 Cr 0.5 SEM image of Zr(PO4)3.
[0033] Figure 4 The precursor Li prepared in Example 1 of the present invention 1.5 Ti 0.5 Cr 0.5 Photo of Zr(PO4)3. DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments are only used to illustrate the present invention, and the protection scope of the present invention is not limited to the specific embodiments, but is defined by the claims.
[0035] The lithium ion sieve according to the present invention is a novel ternary metal lithium ion sieve with a three-dimensional titanium phosphate skeleton top oxygen structure, which is a modified lithium titanium phosphate precursor Li doped with chromium ions and zirconium ions. 1+x Ti y Cr x Zr 2-x-y The delithiation product of (PO4)3, wherein x=0.1-1.4, y=0.4-0.6; Cr 3+ 、Zr 4+ For some Ti 4+ The substitution keeps its framework structure unchanged, improves the ion exchange performance of LiTi2(PO4)3, and then improves the selectivity of ion sieve, and enhances its stability and cyclability.
[0036] Precursor Li 1+x Ti y Cr x Zr 2-x-y (PO4)3 can be prepared by hydrothermal reaction, wherein a mixed solution containing a lithium source, a titanium source, a chromium source, a zirconium source and a phosphorus source is subjected to hydrothermal reaction at a certain temperature, wherein the molar ratio of each metal ion in the titanium source, the chromium source, the zirconium source and the lithium source is Ti 4+ :Cr 3+ :Zr 4+ :Li + =y:x:(2-xy):(1+x), the molar ratio of titanium source to phosphorus source Ti4+ :PO4 3- =y:3; After the hydrothermal reaction product is calcined, the precursor is obtained. The preparation of the mixed solution of the hydrothermal reaction can use water, ethanol or water and ethanol as solvents according to the properties of each raw material. Each raw material can be mixed once or in steps to obtain the mixed solution of the hydrothermal reaction. When preparing the mixed solution, it is recommended to add citric acid to assist dissolution.
[0037] For example, a specific method for preparing the precursor is to mix the titanium source, the chromium source, the zirconium source and the phosphorus source in a molar ratio of Ti 4+ :Cr 3 + :Zr 4+ :PO4 3- =y:x:2-xy:3 is added to the citric acid aqueous solution to prepare a mixed solution, and the lithium source and ethanol are prepared into a lithium solution, wherein the molar ratio of the lithium source is Ti 4+ :Li + =y:(1+x); the lithium solution is added dropwise to the mixed solution, a hydrothermal reaction occurs at 120-180°C, the reaction product is dried, ground and calcined in a muffle furnace, and the calcined product is the ion sieve precursor (L-TCZP).
[0038] In the following examples, the specific method for preparing the precursor is to prepare the titanium source, the chromium source, the zirconium source and the lithium source according to the molar ratio of each metal ion Ti 4+ :Cr 3+ :Zr 4+ :Li + =y:x:(2-xy):(1+x), the molar ratio of titanium source to phosphorus source Ti 4+ :PO4 3- =y:3 Weigh the reaction raw materials, dissolve the titanium source in anhydrous ethanol, add citric acid aqueous solution dropwise, and stir to obtain a transparent titanium citrate solution; add a lithium source, a phosphorus source and a citric acid aqueous solution to the titanium citrate solution, add a chromium source and a zirconium source after stirring, add citric acid aqueous solution, and stir until the transparent solution becomes milky white; subject the obtained mixed solution to a hydrothermal reaction at 120-180° C., dry the reaction product, grind it, and calcine it in a muffle furnace, and the calcined product is the ion sieve precursor (L-TCZP).
[0039] Example 1
[0040] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=0.5, y=0.5) and a preparation method thereof, comprising the following steps:
[0041] According to Li, Zr, Cr, Ti and PO4 3-The raw materials were accurately weighed according to the stoichiometric ratio of 1.5:1:0.5:0.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0042] First, 9.68g (50.4mmol) of citric acid was dissolved in 100mL of deionized water, and 1.23g (3.6mmol) of tetrabutyl titanate was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the tetrabutyl titanate solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then 0.74g (10.8mmol) of LiNO3, 2.50g (21.6mmol) of NH4H2PO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 3.09g (7.2mmol) of Zr (NO3) 4 · 5H2O and 1.44g (3.6mmol) of Cr (NO3) 3 · 9H2O were added, and then 25mL of citric acid solution was added until the transparent solution became milky white and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reaction vessel and subjected to hydrothermal treatment at 150 °C for 24 hours under autogenous pressure. After the reaction was completed, the solution was naturally cooled to room temperature. The powder obtained after filtration and drying was ground and then transferred to a box furnace, first calcined at 500 °C for 4 hours and then heated to 800 °C for 2 hours. The resulting powder is the ion sieve precursor L-TCZP, denoted as Li 1.5 Ti 0.5 Cr 0.5 Zr(PO4)3. Finally, the precursor powder is acid-washed to obtain a ternary lithium ion sieve (HTiCrZr(PO4)3) doped with chromium ions and zirconium ions, which has a three-dimensional [Ti2(PO4)3] - Skeleton, denoted as HTi 0.5 Cr 0.5 Zr(PO4)3.
[0043] The prepared ion sieve precursor and ion sieve were characterized by XRD, and the results were as follows: Figure 1 and Figure 2 As shown in the figure, they all show a good Nasicon structure, the characteristic peaks are well matched and have high intensity, and the crystal stability is good. The ion sieve precursor was characterized by SEM, and the results are shown in the figure. Figure 3 As shown in the figure, the powder particles are small in size and have no obvious agglomeration. Figure 4 .
[0044] The results of ICP measurement showed that the adsorption capacity of the prepared ion sieve was 36.34 mg / g. After 4 cycles of adsorption (repeated delithiation 5 times), the adsorption capacity dropped to 32.86 mg / g, and the titanium dissolution loss was 1.1%.
[0045] Example 2
[0046] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=0.5, y=0.4) and a preparation method thereof, comprising the following steps:
[0047] According to Li, Zr, Cr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 1.5:1.1:0.5:0.4:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0048] First, 11.30g (58.8mmol) of citric acid was dissolved in 100mL of deionized water, and 1.16g (3.4mmol) of tetrabutyl titanate was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the tetrabutyl titanate solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then, 0.87g (12.6mmol) of LiNO3, 3.33g (25.2mmol) (NH4) 2HPO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 3.97g (9.24mmol) of Zr (NO3) 4 · 5H2O and 0.47g (4.2mmol) of Cr2 (CO3) 3 (chromium carbonate) were added, followed by 25mL of citric acid solution, until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 150 ° C for 36 hours under autogenous pressure. After the reaction was completed, the solution was naturally cooled to room temperature. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 550 ° C for 4 hours and then heated to 1000 ° C for 2 hours. The resulting powder was an ion sieve precursor (L-TCZP) with a small powder particle size and no obvious agglomeration. Finally, the precursor powder was acid-washed to obtain a three-dimensional [Ti2(PO4)3] doped with chromium ions and zirconium ions. - Framework ion sieve (HTiCrZr(PO4)3).
[0049] The XRD results of the obtained ion sieve precursor and ion sieve showed a good Nasicon structure. The ICP measurement results showed that the adsorption capacity of the ion sieve was 21.18 mg / g. After 4 cycles of adsorption, the adsorption capacity dropped to 17.62 mg / g, and the titanium dissolution loss was 4.1%.
[0050] Example 3
[0051] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=0.5, y=0.6) and a preparation method thereof, comprising the following steps:
[0052] According to Li, Zr, Cr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 1.5:0.9:0.5:0.6:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0053] First, 11.30g (58.8mmol) of citric acid was dissolved in 100mL of deionized water, and 1.70g (5.0mmol) of tetrabutyl titanate was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the tetrabutyl titanate solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then, 0.87g (12.6mmol) of LiNO3, 3.33g (25.2mmol) (NH4) 2HPO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 2.45g (7.6mmol) of ZrOCl2 · 8H2O (zirconium oxychloride) and 1.68g (4.2mmol) of Cr (NO3) 3 · 9H2O were added, followed by 25mL of citric acid solution, until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 150 ° C for 36 hours under autogenous pressure. After the reaction was completed, the solution was naturally cooled to room temperature. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 550 ° C for 4 hours and then heated to 1000 ° C for 2 hours. The resulting powder was an ion sieve precursor (L-TCZP) with a small powder particle size and no obvious agglomeration. Finally, the precursor powder was acid-washed to obtain a three-dimensional [Ti2(PO4)3] doped with chromium ions and zirconium ions. - Framework ion sieve (HTiCrZr(PO4)3).
[0054] The XRD results of the obtained ion sieve precursor and ion sieve showed a good Nasicon structure. The ICP measurement results showed that the adsorption capacity of the ion sieve was 19.18 mg / g. After 4 cycles of adsorption, the adsorption capacity dropped to 16.62 mg / g, and the titanium dissolution loss was 4.1%.
[0055] Example 4
[0056] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=0.2, y=0.5) and a preparation method thereof, comprising the following steps:
[0057] According to Li, Zr, Cr, Ti and PO4 3+The raw materials were accurately weighed according to the stoichiometric ratio of 1.2:1.3:0.2:0.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0058] First, 14.76g (76.8mmol) of citric acid was dissolved in 100mL of deionized water, and 2.41g (6.0mmol) of Ti (SO4) 2 9H2O was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the above solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then, 1g (14.4mmol) of LiNO3, 3.53g (36.0mmol) of H3PO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 5.06g (15.6mmol) of ZrOCl2 8H2O (zirconium oxychloride) and 0.38g (2.4mmol) of CrCl3 (chromium chloride) were added, and then 25mL of citric acid solution was added until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 120°C for 12 hours under autogenous pressure. After the reaction was completed, the solution was naturally cooled to room temperature. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 300°C for 4 hours and then heated to 600°C for 2 hours. The resulting powder was an ion sieve precursor (L-TCZP) with a small powder particle size and no obvious agglomeration. Finally, the precursor powder was acid-washed to obtain a three-dimensional [Ti2(PO4)3] doped with chromium ions and zirconium ions. - Framework ion sieve (HTiCrZr(PO4)3).
[0059] The XRD of the prepared ion sieve precursor and ion sieve showed a good Nasicon structure. The ICP measurement results showed that the adsorption capacity of the ion sieve was 16.31 mg / g. After 4 cycles of adsorption, the adsorption capacity dropped to 14.86 mg / g, and the titanium dissolution loss was 2.2%.
[0060] Example 5
[0061] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=0.8, y=0.5) and a preparation method thereof, comprising the following steps:
[0062] According to Li, Zr, Cr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 1.8:0.7:0.8:0.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0063] First, 11.68g (60.8mmol) of citric acid was dissolved in 100mL of deionized water, and 1.20g (4.0mmol) of Ti (NO3) 4 was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then 1g (14.4mmol) of LiNO3, 3.29g (24mmol) (NH4) H2PO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 1.59g (5.6mmol) of Zr (SO4) 2 (zirconium sulfate) and 1.25g (3.2mmol) of Cr2 (SO4) 3 were added, and 25mL of citric acid solution was subsequently added until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 140 ° C for 16 hours under autogenous pressure. After the reaction was completed, the solution was naturally cooled to room temperature. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 350 ° C for 4 hours and then heated to 700 ° C for 2 hours. The resulting powder was an ion sieve precursor (L-TCZP) with a small powder particle size and no obvious agglomeration. Finally, the precursor powder was acid-washed to obtain a three-dimensional [Ti2(PO4)3] doped with chromium ions and zirconium ions. - Framework ion sieve (HTiCrZr(PO4)3).
[0064] The XRD of the prepared ion sieve precursor and ion sieve showed a good Nasicon structure. The ICP measurement results showed that the adsorption capacity of the ion sieve was 19.21 mg / g. After 4 cycles of adsorption, the adsorption capacity dropped to 12.13 mg / g, and the titanium dissolution loss was 4.1%.
[0065] Example 6
[0066] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=1.0, y=0.5) and a preparation method thereof, comprising the following steps:
[0067] According to Li, Zr, Cr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 2:0.5:1:0.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0068] First, 11.07g (57.6mmol) of citric acid was dissolved in 100mL of deionized water, and 0.39 (3.6mmol) of Ti (C2H3O2) 4 was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then 1g (14.4mmol) of LiNO3, 3.57g (21.6mol) of Na3PO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 3.71g (3.6mmol) of C6H8O7Zr (citrate zirconium) and 3.01g (7.2mmol) of Cr (C6H4NO2) 3 (nicotinate chromium) were added, and then 25mL of citric acid solution was added until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high pressure reaction vessel and subjected to hydrothermal treatment at 160 ° C for 20 hours under autogenous pressure. After the reaction was completed, the solution was cooled to room temperature naturally. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 400 ° C for 4 hours and then heated to 800 ° C for 2 hours. The resulting powder was an ion sieve precursor (L-TCZP).
[0069] XRD characterization of the prepared ion sieve precursor and ion sieve showed good Nasicon structure, good matching of characteristic peaks and high intensity, and good crystal stability. SEM results showed that the powder particles were small in size and had no obvious agglomeration. ICP measurement showed that the adsorption capacity of the ion sieve was 18.71 mg / g. After 4 cycles of adsorption, the adsorption capacity dropped to 17.36 mg / g, and the dissolution loss of titanium was 3.8%.
[0070] Example 7
[0071] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=1.2, y=0.5) and a preparation method thereof, comprising the following steps:
[0072] According to Li, Zr, Cr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 2.2:0.3:1.2:0.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 1:1.
[0073] First, 10.65g (55.4mmol) of citric acid was dissolved in 100mL of deionized water, and 1.12g (3.3mmol) of tetrabutyl titanate was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the tetrabutyl titanate solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then, 1g (14.5mmol) of LiNO3, 3.07g (9.9mmol) of Ca (H2PO4)2 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 0.33g (2.0mmol) of C3H5O2Zr (zirconium propionate) and 1.72g (7.9mmol) of Cr (CH3COO)3 (chromium acetate) were added, and then 25mL of citric acid solution was added until the transparent solution became milky white and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 180 ° C for 28 hours under autogenous pressure. After the reaction was completed, the solution was naturally cooled to room temperature. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 450 ° C for 4 hours and then heated to 900 ° C for 2 hours. The resulting powder is an ion sieve precursor (L-TCZP), and the powder particles are small in size and have no obvious agglomeration. Finally, the precursor powder was acid-washed to obtain a three-dimensional [Ti2(PO4)3] doped with chromium ions and zirconium ions. - Framework ion sieve (HTiCrZr(PO4)3).
[0074] The XRD of the ion sieve precursor and ion sieve showed a good Nasicon structure. The ICP measurement results showed that the adsorption capacity of the ion sieve was 19.55 mg / g. After 4 cycles of adsorption, the adsorption capacity dropped to 15.34 mg / g, and the loss of manganese was 2.9%.
[0075] Example 8
[0076] A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve (x=1.4, y=0.5) and a preparation method thereof, comprising the following steps:
[0077] According to Li, Zr, Cr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 2.4:0.1:1.4:0.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0078] First, 10.14g (52.8mmol) of citric acid was dissolved in 100mL of deionized water, and 1.02g (3.0mmol) of tetrabutyl titanate was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the tetrabutyl titanate solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then, 1g (14.4mmol) of LiNO3, 4.89g (18mmol) (NH4) 2HPO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 0.62g (0.6mmol) of C6H8O7Zr (citrate zirconium) and 1.19g (4.2mmol) of Cr2 (CO3) 3 (chromium carbonate) were added, followed by 25mL of citric acid solution, until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 150 ° C for 36 hours under autogenous pressure. After the reaction was completed, the solution was naturally cooled to room temperature. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 550 ° C for 4 hours and then heated to 1000 ° C for 2 hours. The resulting powder was an ion sieve precursor (L-TCZP) with a small powder particle size and no obvious agglomeration. Finally, the precursor powder was acid-washed to obtain a three-dimensional [Ti2(PO4)3] doped with chromium ions and zirconium ions. - Framework ion sieve (HTiCrZr(PO4)3).
[0079] The XRD results of the obtained ion sieve precursor and ion sieve showed a good Nasicon structure. The ICP measurement results showed that the adsorption capacity of the ion sieve was 15.16 mg / g. After 4 cycles of adsorption, the adsorption capacity dropped to 11.62 mg / g, and the titanium dissolution loss was 4.1%.
[0080] Comparative Example 1
[0081] A lithium ion sieve (x=0, Ti 2+ / Zr 3+ =1:3) and a preparation method thereof, comprising the following steps:
[0082] According to Li, Zr, Ti and PO4 3- The raw materials were accurately weighed according to the stoichiometric ratio of 1:1.5:0.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0083] First, 16.72g (87mmol) of citric acid was dissolved in 100mL of deionized water, and 2.47g (7.3mmol) of tetrabutyl titanate was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the solution and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then 1g (14.5mmol) of LiNO3, 5.00g (43.5mmol) of NH4H2PO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 9.15g (21.3mmol) of Zr (NO3) 4 · 5H2O was added, followed by 25mL of citric acid solution until the transparent solution became milky white and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 150°C for 24 hours under autogenous pressure. After the reaction was completed, the solution was cooled naturally to room temperature. The filtered and dried powder was ground and then transferred to a box furnace, first calcined at 500°C for 4 hours and then heated to 800°C for 2 hours to remove organic compounds. The resulting ion sieve precursor powder is called L-TZP powder, which has a small particle size and no obvious agglomeration. Finally, the precursor powder was acid-washed to obtain an ion sieve doped with metal zirconium ions.
[0084] The ICP measurement results show that the adsorption capacity of the ion sieve is 15.33 mg / g. After 4 cycles of adsorption, the adsorption capacity drops to 11.31 mg / g, and the titanium dissolution loss is 2.5%.
[0085] Comparative Example 2
[0086] A lithium ion sieve (x=0, Ti 2+ / Zr 3+ =1:9) and a preparation method thereof, comprising the following steps:
[0087] According to Li, Zr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 1:1.8:0.2:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0088] First, 4.8 g (25 mmol) of citric acid was dissolved in 100 mL of deionized water, and 2.09 g (26.1 mmol) of titanium dioxide was dissolved in 20 mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50 mL) was added dropwise to the solution and stirred continuously at 80 ° C for 8 hours to obtain a transparent titanium citrate solution. Then 1 g (14.5 mmol) of LiNO3, 4.17 g (43.5 mmol) of H3PO4 and 25 mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 5.06 g (15.7 mmol) of ZrOCl2·8H2O (zirconium oxychloride) was added, followed by 25 mL of citric acid solution until the transparent solution turned milky white, and stirred at room temperature for 1 h. The resulting mixture was then transferred to a high-pressure reaction vessel containing a 100 mL polytetrafluoroethylene liner and hydrothermally treated at 120 ° C for 12 hours under autogenous pressure. After the reaction was completed, the solution was cooled naturally to room temperature. The dried powder is filtered and ground, then transferred to a box furnace, first calcined at 300°C for 4 hours in the atmosphere, and then heated to 600°C for 2 hours. The resulting ion sieve precursor powder is called L-TZP powder, and the powder particles are small in size and have no obvious agglomeration. Finally, the precursor powder is acid-washed to obtain an ion sieve doped with metal zirconium ions.
[0089] The ICP measurement results show that the adsorption capacity of the ion sieve is 10.41 mg / g. After 4 cycles of adsorption, the adsorption capacity drops to 8.55 mg / g, and the titanium dissolution loss is 3.1%.
[0090] Comparative Example 3
[0091] A lithium ion sieve (x=0, Ti 2+ / Zr 3+ =3:1) and a preparation method thereof, comprising the following steps:
[0092] According to Li, Zr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 1:0.5:1.5:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0093] First, 11.99g (62.4mmol) of citric acid was dissolved in 100mL of deionized water, and 2.96g (15.6mmol) of Ti (NO3) 4 was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then, 0.72g (10.4mmol) of LiNO3, 4.25g (31.2mmol) of KH2PO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 1.47g (5.2mmol) of Zr (SO4) 2 (zirconium sulfate) was added, and then 25mL of citric acid solution was added until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 140°C for 16 hours under autogenous pressure. After the reaction was completed, the solution was cooled to room temperature naturally. The filtered and dried powder is ground and then transferred to a box furnace, first calcined at 350°C for 4 hours, and then heated to 700°C for 2 hours. The resulting ion sieve precursor powder is called L-TZP powder, which has a small particle size and no obvious agglomeration. Finally, the precursor powder is acid-washed to obtain an ion sieve doped with metal zirconium ions.
[0094] The ICP measurement results show that the adsorption capacity of the ion sieve is 12.21 mg / g. After 4 cycles of adsorption, the adsorption capacity drops to 9.73 mg / g, and the titanium dissolution loss is 2.3%.
[0095] Comparative Example 4
[0096] A lithium ion sieve (x=0, Ti 2+ / Zr 3+ =9:1) and a preparation method thereof, comprising the following steps:
[0097] According to Li, Zr, Ti and PO4 3+ The raw materials were accurately weighed according to the stoichiometric ratio of 1:0.2:1.8:3, and the citric acid was weighed according to the molar ratio of metal cations to citric acid of 2:1.
[0098] First, 11.53g (60mmol) of citric acid was dissolved in 100mL of deionized water, and 4.63g (18mmol) of Ti (C2H3O2) 4 was dissolved in 20mL of anhydrous ethanol. Next, half of the citric acid aqueous solution (50mL) was added dropwise to the solution, and stirred continuously at 80°C for 8 hours to obtain a transparent titanium citrate solution. Then 0.69g (10mmol) of LiNO3, 11.40g (30mmol) of Na3PO4 and 25mL of citric acid solution were added to the solution, the mixture was stirred for 30 minutes, 0.48g (2.0mmol) of C3H5O2Zr (zirconium propionate) was added, and then 25mL of citric acid solution was added until the transparent solution became milky white, and stirred at room temperature for 1h. The resulting mixture was then transferred to a 100mL polytetrafluoroethylene-lined high-pressure reaction vessel and hydrothermally treated at 160°C for 20 hours under autogenous pressure. After the reaction was completed, the solution was cooled to room temperature naturally. The filtered and dried powder is ground and then transferred to a box furnace, first calcined at 400°C for 4 hours and then heated to 800°C for 2 hours to remove organic compounds. The resulting ion sieve precursor powder is called L-TZP powder, which has a small particle size and no obvious agglomeration. Finally, the precursor powder is acid-washed to obtain an ion sieve doped with metal zirconium ions.
[0099] The ICP measurement results show that the adsorption capacity of the ion sieve is 13.31 mg / g. After 4 cycles of adsorption, the adsorption capacity drops to 7.66 mg / g, and the titanium dissolution loss is 3.1%.
Claims
1. A three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve, characterized in that: The present invention is a delithiation product of a modified lithium titanium phosphate precursor doped with chromium ions and zirconium ions, wherein the molecular formula of the modified lithium titanium phosphate is Li 1+x Ti y Cr x Zr 2-x-y (PO4)3, wherein x = 0.1-1.4, y = 0.4-0.
6.
2. The lithium ion sieve according to claim 1, characterized in that: In the molecular formula of the modified lithium titanium phosphate, x=0.3-1.2, y=0.4-0.
6.
3. The lithium ion sieve according to claim 1 or 2, characterized in that: The lithium ion sieve has a three-dimensional [Ti2(PO4)3] composed of common apex oxygen - Skeleton, including Cr 3+ 、Zr 4+ Replace part of Ti 4+ .
4. A method for preparing a three-dimensional titanium phosphate framework top oxygen-co-type lithium ion sieve, characterized in that: A lithium source, a titanium source, a chromium source, a zirconium source and a phosphorus source are dissolved in a solvent and mixed, and the resulting mixed solution is subjected to a hydrothermal reaction, wherein the molar ratio of each metal ion in the titanium source, the chromium source, the zirconium source and the lithium source is Ti 4+ :Cr 3+ :Zr 4+ :Li + =y:x:(2-xy):(1+x), the molar ratio of titanium source to phosphorus source Ti 4+ :PO4 3- =y:3; After the hydrothermal reaction product is calcined, a modified lithium titanium phosphate precursor doped with chromium ions and zirconium ions is obtained, and the molecular formula is Li 1+x Ti y Cr x Zr 2-x-y (PO4)3, wherein x=0.1-1.4, y=0.4-0.6; the precursor is delithiated to obtain the lithium ion sieve.
5. The method for preparing a lithium ion sieve according to claim 4, characterized in that: The titanium source is selected from tetrabutyl titanate, tetraisopropyl titanate, titanium acetate, titanium nitrate, titanium sulfate, titanium chloride, titanium dioxide, and titanic acid; The zirconium source is selected from zirconium nitrate, zirconium oxychloride, zirconium citrate, zirconium sulfate, zirconium propionate, or hydrates thereof; The chromium source is selected from chromium nitrate, chromium hydrochloride, chromium sulfate, chromium carbonate, acetyl chromium, chromium nicotinate, or hydrates thereof; The lithium source is selected from lithium nitrate, lithium hydroxide or lithium carbonate; The phosphorus source is selected from phosphoric acid, hydrogen phosphate, dihydrogen phosphate or orthophosphate.
6. The method for preparing a lithium ion sieve according to claim 4, characterized in that: The solvent of the mixed solution is water, ethanol or a mixture of water and ethanol.
7. The method for preparing a lithium ion sieve according to claim 4, characterized in that: The concentration of metal ions in the mixed solution is 0.1-10 mol / L.
8. The method for preparing a lithium ion sieve according to claim 4, characterized in that: The temperature of the hydrothermal reaction is 120° C.-180° C., and the time of the hydrothermal reaction is 12-36 hours.
9. The method for preparing a lithium ion sieve according to claim 4, characterized in that: The calcination temperature is 200-1200° C., and the calcination time is 6-24 hours.
10. The method for preparing a lithium ion sieve according to claim 4, characterized in that: The precursor is delithiated by acid leaching, and the acid for delithiation is selected from hydrochloric acid, sulfuric acid, phosphoric acid, oxalic acid, nitric acid, formic acid, or acetic acid; the concentration of the acid solution is 0.04-0.10 mol / L, and the immersion time is 24h-72h.