A method for treating water leakage from concrete cracks

By using the verified grouting material test and statistical analysis to determine the optimal setting time in concrete crack treatment, and adding accelerators to shorten the setting time of the polyurethane grouting material, the problem of material waste and low treatment quality caused by the long setting time of the polyurethane grouting material is solved. problem, achieving targeted treatment and high-quality water leakage repair.

CN115977417BActive Publication Date: 2024-10-01CHINA WEST CONSTR GRP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211632182.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-10-01
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

Among the existing concrete crack treatment methods, the polyurethane grouting material takes a long time to solidify, resulting in material waste and low treatment quality, and it is impossible to customize the treatment according to different crack characteristics.

Method used

By using a verification grouting material with a viscosity deviation of not more than 10% from the polyurethane grouting material to test the actual filling time of the cracks, statistical analysis determines the optimal setting time, and adding accelerators to shorten the setting time of the polyurethane grouting material to achieve targeted treatment and Improve the quality of governance.

Benefits of technology

It effectively shortens the setting time of polyurethane grouting material, improves the quality of leakage water treatment, reduces material waste, and improves the strength and adhesion of the consolidated body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004006227420000091
    Figure BDA0004006227420000091
Patent Text Reader

Abstract

The present invention provides a method for treating water leakage in concrete cracks, which belongs to the technical field of grouting repair construction for building water leakage. The method comprises the following steps: 1) determining the grouting position and the number of grouting holes; 2) drilling holes and installing grouting nozzles, injecting verification grouting liquid into the leakage part, and recording the overflow time; 3) statistically analyzing and determining the optimal solidification time T of the slurry in the cracks g ; 4) Adjust the setting time T of the polyurethane grouting material g ’ , so that T g ≤T g ’ <T g +10; 5) completing grouting and supplementary injection; 6) after the leakage site is treated until there is no water seepage, removing the grouting nozzle and treating the surface; the method carries out grouting treatment according to the characteristics of the cracks, effectively improving the effect of water leakage treatment of concrete cracks, enabling the polyurethane grouting material to achieve optimal filling and curing in the cracks, and reducing the waste of raw materials during the treatment process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for treating water leakage from concrete cracks, and belongs to the technical field of grouting repair construction for building water leakage. Background Art

[0002] Concrete cracks are a common defect in construction projects. The causes of cracks include defects in concrete mix design, non-standard construction and complex geological environmental factors. Once cracks appear in a building, problems such as water leakage and steel corrosion are very likely to occur, endangering the safety of the structure and must be dealt with in a timely manner.

[0003] At present, injecting polyurethane materials into building cracks and sealing the cracks after solidification is one of the commonly used methods for treating water seepage in concrete cracks. The main problems with this treatment method are: the grouting material used is a universal product with a long solidification time (5-8 minutes), and the solidified body fully reacts and foams (expands ≥20 times), resulting in low body strength (≤5MPa) and low concrete bonding strength (≤0.2MPa), and it is impossible to carry out customized grouting treatment according to the characteristics of the cracks; at the same time, for cracks in the top plate and side walls, the injected polyurethane slurry has a long curing time, and a large amount of slurry is lost due to gravity, which not only causes material waste but also reduces the treatment quality. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for treating water leakage in concrete cracks. The method first uses a verification grouting material with a viscosity deviation of no more than 10% from that of the polyurethane grouting material to replace the polyurethane grouting material, and tests the actual filling time of the slurry in the cracks; then, through statistical analysis, the optimal solidification time of the slurry in the cracks is determined in a targeted manner; then, the solidification time of the polyurethane grouting material is shortened to the optimal solidification time by adding an accelerator, so that the solidification time of the polyurethane slurry is adapted to the actual disease, thereby achieving targeted disease treatment; at the same time, shortening the solidification time can improve the performance of the polyurethane consolidation body, thereby improving the quality of water leakage treatment and reducing material waste in the treatment process.

[0005] The objectives of the present invention are achieved through the following technical solutions.

[0006] A method for treating water leakage in concrete cracks, the method comprising the following steps:

[0007] Step 1: clean the pollutants and loose surface around the cracks, determine the grouting position and the number of grouting holes n, where n is a positive integer ≥ 1;

[0008] Step 2: Drill holes at the grouting locations determined in step 1 and install grouting nozzles. Inject verification grouting liquid into the grouting nozzles and record the time (overflow time) T1 to T2 in each grouting hole from the start of grouting to the time when verification grouting liquid overflows from the cracks.n ;

[0009] The verification grouting liquid is prepared from natural pigment, thickener and water, and the deviation between the viscosity of the verification grouting liquid and the viscosity of the polyurethane grouting material is not more than 10%; wherein the thickener is hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose or carboxymethyl cellulose;

[0010] Step 3: Use the verification slurry to inject the overflow time T1 to T2 obtained in step 2 n Statistical analysis is performed to obtain the optimal setting time T of the polyurethane grouting material in the concrete cracks. g ;

[0011] The statistical analysis methods were:

[0012] S1: Calculate T1~T n The mean value μ, standard deviation σ, and maximum value T max and range R;

[0013] S2: When R≤20s, the optimal solidification time T of the slurry g =T max +σ;

[0014] When R>20s, remove |T n -μ| The grouting hole corresponding to the maximum value, and then repeat step S1 until R ≤ 20s, and then according to T g =T max +σ to obtain the optimal solidification time T of the slurry g ;

[0015] Step 4: Optimal setting time T of the slurry determined in step 3 g Adjust the setting time T of polyurethane grouting material g ’ , so that T g ≤T g ’ <T g +10;

[0016] Step 5: Continue from the grouting hole on one side of the crack to the grouting hole on the other side, and inject the grout from bottom to top through the grouting nozzle. The solidification time obtained after adjustment in step 4 is T g ’ The polyurethane grouting material is used to complete the grouting; if the grouting hole is removed in step three, the verification grouting liquid is injected into the removed grouting hole to obtain the optimal solidification time of the polyurethane slurry in the grouting hole, and then the solidification time of the polyurethane grouting material is adjusted to the optimal solidification time, and the removed grouting hole is supplemented with grouting;

[0017] Step 6. After the polyurethane grouting material solidifies, observe the leaking part with the naked eye to see if there is any water seepage; if there is no water seepage at the leaking part, remove the grouting nozzle and perform surface treatment; if there is still water seepage at the leaking part, repeat steps 2 to 5 to perform additional grouting until there is no water seepage at the leaking part and the treatment requirements are met.

[0018] Furthermore, the method for determining the position and number of the grouting holes in step 1 is as follows: for water leakage with cracks that are invisible to the naked eye, the position of the grouting holes is determined as the center point of the water leakage position;

[0019] For water leakage from cracks visible to the naked eye, the grouting holes are located alternately and evenly along both sides of the cracks, with adjacent grouting holes spaced 5 to 40 cm apart and 1 to 20 cm away from the cracks;

[0020] Furthermore, for water leakage from cracks visible to the naked eye, the grouting holes are determined to be evenly distributed alternately along both sides of the cracks, and the positions of adjacent grouting holes are 10 to 20 cm apart and 5 to 10 cm away from the cracks;

[0021] Furthermore, the hole-making method in step 2 is: for cracks that are invisible to the naked eye, the hole-making depth is 1 / 3 to 2 / 3 of the total thickness of the repaired part where the crack is located;

[0022] For cracks visible to the naked eye, the hole direction is inclined 30 to 60 degrees with the horizontal plane and penetrates the crack. The hole depth is 1 / 3 to 2 / 3 of the total thickness of the repaired part where the crack is located;

[0023] Furthermore, for cracks visible to the naked eye, the hole opening direction is inclined at 45° to the horizontal plane, and the hole opening depth is 2 / 3 of the total thickness of the repaired part where the crack is located;

[0024] Furthermore, in the step 4, the method for adjusting the setting time of the polyurethane grouting material is: adding an accelerator to the polyurethane grouting material, adjusting the amount of the accelerator through experiments and recording the corresponding slurry setting time data until the setting time T of the polyurethane grouting material is adjusted to g ’ Meet T g ≤T g ’ <T g +10;

[0025] The accelerator is dibutyltin dilaurate, stannous octoate, potassium isooctanoate, bismuth isooctanoate or bismuth neodecanoate.

[0026] Beneficial Effects

[0027] (1) The present invention provides a method for treating water leakage in concrete cracks. The method carries out targeted grouting treatment according to the characteristics of the cracks. A slurry with a viscosity deviation of 10% from the polyurethane grouting material is first prepared as a verification grouting material, which is used to replace the general polyurethane grouting material to test the actual setting time of the cracks and perform statistical analysis. The statistical analysis method can effectively determine the optimal setting time T of the slurry required for the concrete cracks. g ; Then the setting time T of the general polyurethane grouting material g ’ Make targeted adjustments so that the relationship between its coagulation time and the optimal coagulation time satisfies T g ≤T g ’ <T g +10, in order to achieve the best filling and curing of polyurethane grouting material in the cracks, effectively improving the effect of concrete crack leakage treatment, while reducing the waste of raw materials in the treatment process.

[0028] (2) The present invention provides a method for treating water leakage in concrete cracks. The method effectively shortens the solidification time of the general grouting material product by adding an accelerator to the general polyurethane grouting material, thereby reducing the foaming degree of the polyurethane grouting material solid body and improving the strength and adhesion of the solid body; for cracks in the top plate and side wall, the method shortens the solidification time of the polyurethane slurry and effectively reduces the material waste and reduced treatment quality caused by the loss of the polyurethane grouting liquid due to gravity.

[0029] (3) The present invention provides a method for treating water leakage in concrete cracks, wherein the verification grouting liquid is prepared from natural pigments, thickeners and water; the natural pigments are convenient for indicating, observing and recording the setting time, and the thickeners can effectively adjust the viscosity of the verification grouting liquid to a viscosity deviation within 10% of that of the general polyurethane grouting liquid, thereby improving the accuracy of the verification experiment; and the components of the verification grouting liquid do not affect the treatment effect of the subsequent polyurethane grouting material, and are environmentally friendly and pollution-free.

[0030] (4) The present invention provides a method for treating water leakage in concrete cracks. The method provides a method for determining the position and number of grouting holes and a method for opening holes, respectively, depending on whether the concrete cracks are visible to the naked eye, thereby improving the quality of treating water leakage in concrete cracks. DETAILED DESCRIPTION

[0031] The present invention is further described below in conjunction with specific embodiments. The methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.

[0032] 1. Raw material information: In the following comparative examples and examples, the raw materials described can be obtained from public commercial channels unless otherwise specified.

[0033] The polyurethane grouting material is a polyurethane consolidation water plugging agent of model DMPU-D-GJ-40 / 30 produced by Demei Company; the setting time of the polyurethane grouting material is 316s, and the slurry viscosity is 540mPa·s.

[0034] 2. Performance test:

[0035] (1) Setting time and foaming rate: Tested according to the recommended standard of the building materials industry "JC / T 2041-2020 Polyurethane Grouting Materials";

[0036] (2) Bond strength: Tested according to the recommended standard of the building materials industry "JC / T 1041-2007 Epoxy Resin Grouting Materials for Concrete Cracks";

[0037] (3) Compressive strength of the polyurethane grouting liquid consolidation body: tested by on-site sampling using the Instron 8874 material testing machine manufactured by Instron Corporation of the United States;

[0038] (4) The loss of polyurethane grouting fluid and the leakage after 90 days: through on-site observation test.

[0039] Example 1

[0040] A method for treating water leakage from concrete cracks, wherein the cracks are micro-leakage sites where cracks cannot be identified, and the leakage area is 0.5m 2 , the crack is located at the top plate of the basement, and the method comprises the following steps:

[0041] Step 1: Clean the pollutants and loose surface around the cracks, determine the locations of the three water seepage centers as grouting locations, and the number of grouting holes is 3;

[0042] Step 2: Drill a hole at the grouting position determined in step 1 and install a grouting nozzle. The hole depth is 1 / 2 of the thickness of the leakage part. Inject verification grouting liquid into the grouting nozzle and record the time T1 to T3 from the start of grouting to the overflow of grouting liquid from the crack in each grouting hole, which are 11s, 15s and 17s respectively.

[0043] The verification grouting liquid is prepared from 0.05g of natural pigment indigo, 0.51g of carboxymethyl cellulose and 100g of water. The viscosity of the verification grouting liquid is 563mPa·s, and the deviation from the viscosity of the polyurethane grouting material is no more than 10%;

[0044] Step 3: Statistically analyze the time T1 to T3 from the start of grouting to the overflow of slurry from the cracks in each grouting hole obtained by grouting the verification slurry in step 2, so as to obtain the optimal solidification time T of the slurry in the concrete cracks. g ;

[0045] The statistical analysis methods were:

[0046] S1: Calculate the average value μ, standard deviation σ, and maximum value T of T1 to T3 max and range R; where μ = 14.3s, σ = 2.5s, T max =17s, R=6s;

[0047] S2: R = 6s < 20s, so the optimal setting time of the slurry in the concrete crack is T g =T max +σ, that is, T g =17s+2.5s=19.5s;

[0048] Step 4: Optimal setting time T of the slurry determined in step 3 g =19.5s, add 0.84g of accelerator dibutyltin silicate to 100g of polyurethane grouting material to adjust the setting time T of polyurethane grouting material g ' = 20s;

[0049] Step 5: Inject the polyurethane grouting material adjusted in step 4 into the leakage part from bottom to top through the grouting nozzles from one side of the crack to the other side of the crack;

[0050] Step 6: After the polyurethane grouting material solidifies, observe whether there is water seepage at the leakage site, remove the grouting nozzle and apply mortar.

[0051] Example 2

[0052] A method for treating water leakage in concrete cracks, wherein the cracks are identifiable water leakage sites, the cracks are located at the concrete side wall, the crack width is 0.15 mm, and the length is 0.9 m, the method comprising the following steps:

[0053] Step 1: Clean the pollutants and loose surface around the cracks, and identify the location and direction of the cracks; alternately and evenly arrange grouting holes on both sides of the cracks, with 5 grouting holes; the spacing between adjacent grouting holes is 20 cm, and the distance between the grouting holes and the cracks is 10 cm;

[0054] Step 2: Drill a hole at the grouting position determined in step 1, the hole depth is 2 / 3 of the thickness of the leakage part, and the hole direction is inclined at 45° to the horizontal plane; use compressed air to clean the dust in the hole and then install the grouting nozzle; inject verification grouting liquid into the grouting nozzle, and record the time from the start of grouting to the overflow of slurry from the cracks in each grouting hole, T1~T5 are 8s, 12s, 9s, 13s and 20s respectively;

[0055] The verification grouting liquid is prepared from 0.5g of natural pigment capsicum orange, 0.57g of hydroxyethyl cellulose and 100g of water. The viscosity of the verification grouting liquid is 547mPa·s, and the deviation from the viscosity of the polyurethane grouting material is no more than 10%;

[0056] Step 3: Statistically analyze the time T1 to T5 from the start of grouting to the overflow of slurry from the cracks in each grouting hole obtained by grouting the verification slurry in step 2, so as to obtain the optimal solidification time T of the slurry in the concrete cracks. g ;

[0057] The statistical analysis methods were:

[0058] S1: Calculate the average value μ, standard deviation σ, and maximum value T of T1 to T5 max and range R; where μ = 12.4s, σ = 4.2s, T max =20s, R = 12s;

[0059] S2: R = 12s < 20s, so the setting time of the polyurethane grouting material is T g =T max +σ, that is, T g =20s+4.2s=24.2s;

[0060] Step 4: Optimal setting time T of the slurry determined in step 3 g = 24.2s, add 0.74g of accelerator stannous octoate to 100g of polyurethane grouting material to adjust the setting time T of the polyurethane grouting material g ’ =30s;

[0061] Step 5: Inject the polyurethane grouting material adjusted in step 4 into the leakage part from bottom to top through the grouting nozzles from one side of the crack to the other side of the crack;

[0062] Step 6: After the polyurethane grouting material solidifies, observe whether there is water seepage at the leakage site, remove the grouting nozzle and apply mortar.

[0063] Example 3

[0064] A method for treating water leakage in concrete cracks, wherein the cracks are identifiable water leakage sites, the cracks are located at the top plate, have a width of 0.5 mm and a length of 1.6 m, and the method comprises the following steps:

[0065] Step 1: Clean the pollutants and loose surface around the cracks, and identify the location and direction of the cracks; alternately and evenly arrange grouting holes on both sides of the cracks, with 12 grouting holes; the spacing between adjacent grouting holes is 10 cm, and the distance between the grouting holes and the cracks is 5 cm;

[0066] Step 2: Drill holes at the grouting positions determined in step 1. The hole depth is 2 / 3 of the thickness of the leaking part, and the hole direction is inclined at 45° to the horizontal plane. Use compressed air to clean the dust in the hole and then install the grouting nozzle. Inject verification grouting liquid into the grouting nozzle, and record the time from the start of grouting to the overflow of grouting liquid from the cracks in each grouting hole, T1~T 12 and 12s, 15s, 11s, 17s, 18s, 25s, 13s, 19s, 10s, 32s, 18s and 14s respectively;

[0067] The verification grouting liquid is prepared from 0.1g of natural pigment gardenia yellow, 0.49g of hydroxypropyl cellulose and 100g of water. The viscosity of the verification grouting liquid is 507mPa·s, and the deviation from the viscosity of the polyurethane grouting material is no more than 10%;

[0068] Step 3: For each grouting hole obtained by grouting with the verification slurry in step 2, the time from the start of grouting to the overflow of slurry from the cracks is T1~T 12 Statistical analysis is performed to obtain the optimal setting time T of the slurry in the concrete cracks. g ;

[0069] The statistical analysis methods were:

[0070] S1: Calculate T1~T 12 The mean value μ, standard deviation σ, and maximum value T max and range R; where μ = 17s, σ = 6.0s, T max =32s, R=22s;

[0071] S2: R=22s>20s, remove |T n -μ| The grouting hole corresponding to the maximum value, that is, T 10 The corresponding grouting hole, then repeat step S1, recalculate the average value μ' = 15.6s, standard deviation σ' = 4.1s, maximum value T' max = 25s and range R' = 15s;

[0072] R'=15s<20s, so according to T g =T max +σ to obtain the setting time T of the polyurethane grouting material g =25s+4.1s=29.1s;

[0073] Step 4: Optimal setting time T of the slurry determined in step 3 g = 29.1s, add 0.9g of accelerator bismuth isooctanoate to 100g of polyurethane grouting material to adjust the setting time T of the polyurethane grouting material g ’=38s;

[0074] Step 5: Inject the polyurethane grouting material adjusted in step 4 into the leakage part from bottom to top through the grouting nozzles from one side of the crack to the other side of the crack;

[0075] Towards the removal point T 10 Inject verification grouting liquid into the corresponding grouting hole to determine the setting time T 10 ; Then adjust the setting time of the polyurethane slurry to T 10 , carry out grouting;

[0076] Step 6: After the polyurethane grouting material solidifies, observe whether there is water seepage at the leakage site, remove the grouting nozzle and apply mortar.

[0077] Comparative Example 1

[0078] A method for treating water leakage from concrete cracks, wherein the cracks are micro-leakage sites where cracks cannot be identified, and the leakage area is 0.5m 2 , the crack is located at the top plate of the basement, and the method comprises the following steps:

[0079] Step 1: Clean the pollutants and loose surface around the cracks, determine the locations of the three water seepage centers as grouting locations, and the number of grouting holes is 3;

[0080] Step 2: Drill a hole at the grouting position determined in step 1 and install a grouting nozzle. The depth of the hole should be 1 / 2 of the thickness of the leaking part.

[0081] Step 3: Inject polyurethane grouting material into the leakage part from bottom to top through the grouting nozzle from one side of the crack to the other side of the crack;

[0082] Step 4: After the polyurethane grouting material solidifies, observe whether there is water seepage at the leakage site, remove the grouting nozzle and apply mortar.

[0083] Comparative Example 2

[0084] A method for treating water leakage in concrete cracks, wherein the cracks are identifiable water leakage sites, the cracks are located at the concrete side wall, the crack width is 0.15 mm, and the length is 0.9 m, the method comprising the following steps:

[0085] Step 1: Clean the pollutants and loose surface around the cracks, and identify the location and direction of the cracks; alternately and evenly arrange grouting holes on both sides of the cracks, with 5 grouting holes; the spacing between adjacent grouting holes is 20 cm, and the distance between the grouting holes and the cracks is 10 cm;

[0086] Step 2: Drill a hole at the grouting position determined in step 1, the hole depth is 2 / 3 of the thickness of the leakage part, and the hole direction is inclined at 45° to the horizontal plane; use compressed air to clean the dust in the hole and then install the grouting nozzle;

[0087] Step 3: Inject polyurethane grouting material into the leakage part from bottom to top through the grouting nozzle from one side of the crack to the other side of the crack;

[0088] Step 4: After the polyurethane grouting material solidifies, observe whether there is water seepage at the leakage site, remove the grouting nozzle and apply mortar.

[0089] Comparative Example 3

[0090] A method for treating water leakage in concrete cracks, wherein the cracks are identifiable water leakage sites, the cracks are located at the top plate, have a width of 0.5 mm and a length of 1.6 m, and the method comprises the following steps:

[0091] Step 1: Clean the pollutants and loose surface around the cracks, and identify the location and direction of the cracks; alternately and evenly arrange grouting holes on both sides of the cracks, with 12 grouting holes; the spacing between adjacent grouting holes is 10 cm, and the distance between the grouting holes and the cracks is 5 cm;

[0092] Step 2: Drill a hole at the grouting position determined in step 1, the hole depth is 2 / 3 of the thickness of the leakage part, and the hole direction is inclined at 45° to the horizontal plane; use compressed air to clean the dust in the hole and then install the grouting nozzle;

[0093] Step 3: Inject polyurethane grouting material into the leakage part from bottom to top through the grouting nozzle from one side of the crack to the other side of the crack;

[0094] Step 4: After the polyurethane grouting material solidifies, observe whether there is water seepage at the leakage site, remove the grouting nozzle and apply mortar.

[0095] The performance parameters of the polyurethane grouting materials described in Examples 1 to 3 and Comparative Examples 1 to 3 were tested, and the effect of the method on the treatment of water leakage in concrete cracks was judged by observing the slurry loss and the leakage after 90 days. The results are shown in Table 3, where "-" means that the test was not performed:

[0096] Table 3 Performance parameters and repair effects of the grouting materials described in Examples 1 to 3 and Comparative Examples 1 to 3

[0097]

[0098] The test results show that the treatment method of the present invention can be used to carry out targeted customized repair of concrete cracks, with good repair effect, no leakage within 90 days, low loss of top plate grouting liquid, and less waste of raw materials in the treatment process.

[0099] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for treating water leakage in concrete cracks, characterized in that: The method comprises the following steps: (1) Determine the grouting position and the number of grouting holes n, where n is a positive integer ≥ 1; (2) Drill holes at the grouting location and inject verification grouting liquid, and record the overflow time T1~T of each grouting hole. n ; Verify that the viscosity of the grouting fluid is ≤10% of the viscosity of the polyurethane grouting material, which is composed of natural pigments, thickeners and water; The thickener is hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose or carboxymethyl cellulose; (3) For T1~ T n Perform statistical analysis to determine the optimal solidification time T of the slurry in the crack g ; The statistical analysis methods were: S1: Calculate T1~T n The mean value μ, standard deviation σ, and maximum value T max and range R; S2: When R ≤ 20s, the optimal solidification time T g =T max +σ; When R>20s, remove |T n -μ| The grouting hole corresponding to the maximum value, repeat step S1 to R≤20s, and then according to T g =T max +σ to obtain the optimal solidification time T g ; (4) Adjust the setting time T of polyurethane grouting material g ’ , so that T g ≤T g ’ <T g +10; (5) Inject the adjusted polyurethane grouting material. If the grouting holes are removed, verify the grouting and supplement the grouting of the removed grouting holes; (6) After the polyurethane grouting material solidifies, if there is no water seepage at the leaking part, remove the grouting nozzle and perform surface treatment; if there is still water seepage at the leaking part, repeat steps 2 to 5 to fill the leaking part until there is no water seepage; The method for determining the location and number of grouting holes is as follows: for water leakage from cracks that are invisible to the naked eye, the location of the grouting holes is determined as the center point of the water leakage location; For water leakage from cracks visible to the naked eye, the grouting holes are located alternately and evenly along both sides of the cracks, with adjacent grouting holes spaced 5 to 40 cm apart and 1 to 20 cm away from the cracks; The hole opening method is: for cracks that are invisible to the naked eye, the hole opening depth is 1 / 3~2 / 3 of the total thickness of the repaired part where the crack is located; For cracks visible to the naked eye, the hole opening direction is inclined at 30~60° to the horizontal plane and passes through the crack. The hole opening depth is 1 / 3~2 / 3 of the total thickness of the repaired part where the crack is located.

2. A method for treating water leakage from concrete cracks according to claim 1, characterized in that: For water leakage from cracks visible to the naked eye, the locations of grouting holes are determined to be evenly distributed alternately along both sides of the cracks, with adjacent grouting holes spaced 10 to 20 cm apart and 5 to 10 cm away from the cracks.

3. A method for treating water leakage from concrete cracks according to claim 1, characterized in that: For cracks visible to the naked eye, the hole opening direction is inclined at 45° to the horizontal plane, and the hole opening depth is 2 / 3 of the total thickness of the repaired part where the crack is located.

4. A method for treating water leakage from concrete cracks according to claim 1, characterized in that: For water leakage from cracks visible to the naked eye, the grouting holes are located alternately and evenly along both sides of the cracks, with adjacent grouting holes spaced 10-20 cm apart and 5-10 cm away from the cracks; For cracks visible to the naked eye, the hole opening direction is inclined at 45° to the horizontal plane, and the hole opening depth is 2 / 3 of the total thickness of the repaired part where the crack is located.

5. A method for treating water leakage from concrete cracks according to any one of claims 1 to 4, characterized in that: Polyurethane grouting material setting time T g ’ The adjustment method is: Add accelerator to the polyurethane grouting material, adjust the amount of accelerator through experiments and record the corresponding slurry setting time data until the setting time T of the polyurethane grouting material is adjusted. g ’ Meet T g ≤T g ’ <T g +10; The accelerator is dibutyltin dilaurate, stannous octoate, potassium isooctanoate, bismuth isooctanoate or bismuth neodecanoate.