Laminated bodies and methods for manufacturing laminated bodies

By forming titanium carbide and titanium layers on the resin layer as adhesive layers, the adhesion between the insulating resin layer and the seed crystal layer is improved, solving the problem of insufficient adhesion in traditional methods, and achieving stability and fine wiring formation under high temperature and high humidity environments.

CN115989578BActive Publication Date: 2026-11-17CANON ANELVA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180052501.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-18
Publication Date
2026-11-17
Estimated Expiration
2041-05-18

AI Technical Summary

Technical Problem

In the prior art, the adhesion between the insulating resin layer and the seed crystal layer is insufficient, especially in high temperature and high humidity environments, and traditional methods are not able to form fine wiring to increase the density of semiconductor packages.

Method used

By forming a titanium carbide layer and a titanium layer on the resin layer as an adhesive layer, and combining methods such as ion irradiation or high-frequency voltage to improve the adhesion between the resin layer and the seed crystal layer, a second wiring layer including the adhesive layer and the seed crystal layer is formed.

Benefits of technology

It improves the adhesion between the resin layer and the seed layer, ensures the stability of adhesion under various environments, supports the formation of fine wiring, and improves the reliability of semiconductor packages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115989578B_ABST
    Figure CN115989578B_ABST
Patent Text Reader

Abstract

This invention proposes a laminate that improves the adhesion between a resin layer and a seed layer; and a method for manufacturing the laminate. The laminate sequentially comprises a substrate, a first wiring layer, a resin layer, and a second wiring layer. The second wiring layer sequentially comprises at least an adhesive layer and a seed layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to laminates and methods for manufacturing laminates. Background Technology

[0002] In the mounting step of mounting electronic components onto a substrate including a printed circuit board and a film substrate, an adhesive layer and a seed layer are formed on an insulating resin layer. The adhesive layer is the bottom layer for wiring connected to the electronic components, and the seed layer is used to form the wiring by electroplating. For example, electroplating or sputtering is used to form the respective layers.

[0003] Patent Document 1 discloses a wiring formation method that uses electroless copper plating and provides excellent adhesion and high connection reliability. Furthermore, Patent Document 2 discloses a wiring formation method as a fine wiring formation scheme, which uses a titanium (Ti) / copper (Cu) layer as a seed layer formed by sputtering, a mainstream method that can achieve adhesion to smooth resin surfaces.

[0004] [Existing Technical Documents]

[0005] [Patent Literature]

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-10276

[0007] Patent Document 2: International Publication No. WO2008 / 105535 Summary of the Invention

[0008] The technical problem that the invention aims to solve

[0009] However, in the wiring formation method using electroplating-free method disclosed in Patent Document 1, the surface of the insulating resin layer is roughened to ensure adhesion, and therefore it is difficult to form fine wiring for increasing the density of semiconductor packages due to the uneven surface.

[0010] Furthermore, it is desirable for the wiring layer to maintain adhesion to various insulating resin layers even under various environments such as high temperature and high humidity, i.e., excellent reliability. However, according to the inventors' research, it has been revealed that when using the seed layer made of Ti and Cu layers disclosed in Patent Document 2, it is difficult to obtain sufficient adhesion to various insulating resin layers.

[0011] The present invention was made in view of the above-mentioned problems of the conventional technology, and aims to provide a laminate and a method for manufacturing a laminate that can improve the adhesion between the resin layer and the seed crystal layer.

[0012] Solution for solving the problem

[0013] To achieve the above objectives, a laminate according to one aspect of the present invention sequentially comprises: a first wiring layer; a resin layer; and a second wiring layer, wherein the second wiring layer sequentially comprises at least an adhesive layer and a seed layer.

[0014] A method for manufacturing a laminate according to another aspect of the present invention includes: a first step of forming a titanium film on a resin layer; a second step following the first step of forming a titanium carbide layer by applying energy to the titanium film, the titanium carbide layer forming part of an adhesive layer; a third step following the second step of forming a titanium layer on the titanium carbide layer, the titanium layer forming part of the adhesive layer; and a fourth step following the third step of forming a seed layer on the titanium layer.

[0015] According to another aspect of the present invention, the laminate sequentially comprises: a first wiring layer; a resin layer; and a second wiring layer, the second wiring layer sequentially comprising an adhesive layer and a seed layer, the adhesive layer sequentially comprising a titanium carbide layer and a titanium layer, and the titanium carbide layer being formed by applying energy to a titanium film formed on the resin layer.

[0016] Advantages of the invention

[0017] According to the present invention, the adhesion between the resin layer and the seed crystal layer can be improved. Other features and advantages of the invention will become apparent from the following description with reference to the accompanying drawings. Note that throughout the drawings, the same or similar features are labeled with the same reference numerals. Attached Figure Description

[0018] [ Figure 1 ] Figure 1 This is a schematic cross-sectional view showing the wiring portion of a semiconductor package according to a first embodiment of the present invention.

[0019] [ Figure 2 ] Figure 2 This is a cross-sectional view of the membrane forming apparatus according to the first embodiment of the present invention, taken along a vertical plane.

[0020] [ Figure 3 ] Figure 3 This is a flowchart illustrating a method for manufacturing a laminate according to a first embodiment of the present invention.

[0021] [ Figure 4A ] Figure 4A This is a cross-sectional view showing the steps of a laminate manufacturing method according to a first embodiment of the present invention.

[0022] [ Figure 4B ] Figure 4B This is a cross-sectional view showing the steps of a laminate manufacturing method according to a first embodiment of the present invention.

[0023] [ Figure 4C ] Figure 4C This is a cross-sectional view showing the steps of a laminate manufacturing method according to a first embodiment of the present invention.

[0024] [ Figure 4D ] Figure 4D This is a cross-sectional view showing the steps of a laminate manufacturing method according to a first embodiment of the present invention.

[0025] [ Figure 4E ] Figure 4E This is a cross-sectional view showing the steps of a laminate manufacturing method according to a first embodiment of the present invention.

[0026] [ Figure 5 ] Figure 5 This is a cross-sectional view of the membrane forming apparatus according to the second embodiment of the present invention, taken along a vertical plane.

[0027] [ Figure 6 ] Figure 6 This is a cross-sectional view of the membrane forming apparatus according to the third embodiment of the present invention, taken along a vertical plane.

[0028] [ Figure 7 ] Figure 7 This is a figure showing an example of a C1s spectrum obtained by X-ray photoelectron spectroscopy measurement.

[0029] [ Figure 8 ] Figure 8 This is a figure showing an example of a Ti2p spectrum obtained by X-ray photoelectron spectroscopy.

[0030] [ Figure 9 ] Figure 9 This is a graph showing the measurement results of a 90-degree peel test performed on a laminate obtained in an embodiment of the present invention. Detailed Implementation

[0031] Reference Figures 1 to 9 This describes embodiments of the invention found in the inventors' discoveries.

[0032] [First Implementation Method]

[0033] Reference Figures 1 to 4E A laminate and a method for manufacturing the same according to a first embodiment of the present invention will be described. In this embodiment, a laminate including a wiring layer in the wiring portion of a semiconductor package will be described as a laminate.

[0034] First, refer to Figure 1 The wiring portion of the semiconductor package according to this embodiment is described. Figure 1 This is a schematic cross-sectional view showing the wiring portion of a semiconductor package according to this embodiment. Figure 1As shown, the wiring portion 1 of the semiconductor package sequentially includes a printed wiring substrate 2, a first wiring layer 5, a resin layer 6, and a second wiring layer 7. The wiring portion 1 of the semiconductor package also includes solder 8 and an underfill layer 9.

[0035] The printed wiring substrate 2 is not particularly limited and can be, for example, a known buildup substrate, and has a substrate 3 and wiring 4 disposed on the substrate 3.

[0036] Wiring 4 is a metal layer that forms an inner layer wiring pattern on a stacked substrate, such as a printed wiring substrate 2, and is formed, for example, by electroplating. In terms of electroplating adhesion, conductivity, and cost, copper or a copper alloy is preferably used as the metal layer for wiring 4.

[0037] The first wiring layer 5 is a metal layer formed on the support substrate C, as described later, and is formed, for example, by a semi-additive method. Copper or a copper alloy is preferably used as the metal layer for the first wiring layer 5. The first wiring layer 5 is formed on the surface of the resin layer 6 on the side of the printed wiring substrate 2.

[0038] Resin layer 6 is formed from a cured resin. For example, polyimide-based resin, epoxy-based resin, phenol-based resin, polybenzoxazole-based resin, or fluoropolymer resin can be used as the resin. Resin layer 6 is an insulating resin layer that serves as an interlayer insulating film to insulate conductive layers such as the first wiring layer 5 from each other.

[0039] Wiring 4 and the first wiring layer 5 are electrically connected to each other via solder 8. An underfill material is filled between the printed wiring substrate 2 including the wiring 4 and the resin layer 6 including the first wiring layer 5, forming an underfill layer 9 made of the underfill material.

[0040] The second wiring layer 7 sequentially comprises an adhesive layer 7A, a sputtered seed layer 73, and a copper plating layer 74. The second wiring layer 7 is formed to connect to the first wiring layer 5 through a via 10 formed in the resin layer 6 (including vias 10 formed in the resin layer 6). For example, the via 10 is formed such that a portion of the surface of the first wiring layer 5 is exposed, for example, by patterning a photoresist on the resin layer 6. The second wiring layer 7 is, for example, a wiring formed by a semi-additive method after the adhesive layer and the seed layer are stacked in the opening of the via 10 by sputtering. Note that the second wiring layer 7 can be any layer, as long as it at least sequentially comprises an adhesive layer 7A and a sputtered seed layer 73.

[0041] The second wiring layer 7 is electrically connected to the first wiring layer 5 at the bottom of the via 10. In the second wiring layer 7, a titanium layer 72, a sputtered seed layer 73, and a copper plating layer 74 are sequentially stacked from the side of the first wiring layer 5 at the bottom of the via 10. Furthermore, in the second wiring layer 7, an adhesive layer 7A, a sputtered seed layer 73, and a copper plating layer 74 are sequentially stacked from the side of the resin layer 6, which insulates the first wiring layer 5 and the second wiring layer 7 from each other. The adhesive layer 7A is formed of a titanium carbide layer 71 and a titanium layer 72.

[0042] In this manner, the second wiring layer 7 sequentially comprises a titanium carbide layer 71, a titanium layer 72, a sputtered seed layer 73, and a copper plating layer 74, and is formed as a stacked body connected to the first wiring layer 5 through the via 10. The titanium layer 72, the sputtered seed layer 73, and the copper plating layer 74 are sequentially stacked on the first wiring layer 5 from the side of the first wiring layer 5, such that the first wiring layer 5 and the titanium layer 72 are electrically connected to each other at the bottom of the via 10. At the bottom of the via 10, the titanium layer 72 is formed directly on the first wiring layer 5 without passing through the titanium carbide layer 71. On the other hand, the titanium carbide layer 71, the titanium layer 72, the sputtered seed layer 73, and the copper plating layer 74 are sequentially stacked on the resin layer 6 from the side of the resin layer 6, such that the first wiring layer 5 and the titanium layer 72 are insulated from each other in the portion except at the bottom of the via 10.

[0043] The adhesive layer 7A has a titanium carbide layer 71 and a titanium layer 72 sequentially from the resin layer 6 side. The adhesive layer 7A has a titanium carbide layer 71 on the resin layer 6 side, which has excellent adhesion to the resin layer 6, and a titanium layer 72 on the sputtering seed layer 73 side, which has excellent adhesion to the sputtering seed layer 73.

[0044] The titanium carbide layer 71 is formed from a titanium carbide (TiC) bonding layer. The titanium carbide bonding layer is formed such that, while the titanium film has already been formed on the resin layer 6, energy is applied to it via ion irradiation, thereby covalently bonding the titanium elements contained in the titanium film and the carbon (C) elements contained in the resin layer 6 (hereinafter also referred to as titanium carbide bonding). The thickness of the titanium film used to form the titanium carbide layer 71 is preferably 2.5 nm or greater. Furthermore, the energy of the ions emitted by ion irradiation is preferably 250 eV or greater. In this document, since the titanium carbide layer 71 can be formed even when the titanium film used to form the titanium carbide layer 71 is an extremely thin film with a thickness of 2.5 nm, the titanium carbide layer 71 can be formed without reducing productivity. Furthermore, since the irradiation ion energy of 250 eV allows ions to penetrate several nm or more into the depth direction from the outermost surface of the resin layer 6, the titanium carbide layer 71 can be formed efficiently.

[0045] The titanium layer 72 is formed of titanium (Ti). The film thickness of the titanium layer 72 can be 5 nm or greater, and preferably 20 nm to 200 nm. The titanium layer 72 can be formed, for example, by sputtering a titanium target under an argon (Ar) atmosphere.

[0046] The sputtering seed layer 73 is formed of copper (Cu). The sputtering seed layer 73 is formed on the adhesive layer 7A by sputtering and serves as the seed layer for forming the copper electroplated layer 74. The film thickness of the sputtering seed layer 73 can be 50 nm or greater, preferably 100 nm to 300 nm. For example, the sputtering seed layer 73 can be formed by sputtering a Cu target under an argon atmosphere. In this embodiment, since the sputtering seed layer 73 is formed on the resin layer 6 via the adhesive layer 7A, the adhesion between the resin layer 6 and the sputtering seed layer 73 is improved.

[0047] The copper plating layer 74 is formed of copper (Cu). After the sputtering seed layer 73 is formed, the copper plating layer 74 can be stacked on the sputtering seed layer 73 by electroplating. The thickness of the copper plating layer 74 can be 5 μm or greater, and preferably 10 μm to 50 μm.

[0048] In this manner, a second wiring layer 7 connected to the first wiring layer 5 is formed in the wiring portion 1 of the semiconductor package. The adhesive layer 7A and the sputtering seed layer 73 of the second wiring layer 7 can be formed by using... Figure 2 The membrane forming apparatus shown in this embodiment is a single membrane forming apparatus. Figure 2 This is a cross-sectional view of the film forming apparatus of this embodiment taken along a vertical plane. In this document, the XY plane is a plane parallel to the horizontal plane, and the Z-axis is an axis parallel to the vertical direction.

[0049] like Figure 2As shown, the film forming apparatus according to this embodiment includes a processing chamber 50, a processing unit FF1, an venting unit V50, a gas introduction unit G1, a holding unit 60, and a control device CR. The processing unit FF1 is disposed inside the processing chamber 50 and is configured to form an adhesive layer 7A and a sputtering seed layer 73 for a second wiring layer 7, the second wiring layer corresponding to wiring of electronic components connected to a substrate S. The venting unit V50 is configured to evacuate the processing chamber 50. The gas introduction unit G1 is configured to introduce gas used for forming the adhesive layer 7A and the sputtering seed layer 73 into the processing chamber 50. The holding unit 60 is configured to hold the substrate S in the processing chamber 50. The control device CR is configured to control various units of the film forming apparatus, such as the venting unit V50, the gas introduction unit G1, and the processing unit FF1. Furthermore, the film forming apparatus according to this embodiment has a drive unit (not shown) and a cooling unit (not shown). The drive unit moves the holding unit 60 that holds the substrate S, so that the substrate S travels through the film forming area in the processing chamber 50, and the cooling unit cools the holding unit 60.

[0050] The processing unit FF1 has multiple targets T1 and T2 as sputtering targets and an ion gun I1, and is formed by a rotating cathode that rotates a support SP that supports the multiple targets T1 and T2 and the ion gun I1. Target T1 is, for example, a titanium (Ti) target, and is preferably formed of a material used for an adhesive film formed on a substrate S as an adhesive layer 7A. For example, the processing unit FF1 deposits a titanium film using target T1 by sputtering. Target T2 is, for example, a copper (Cu) target, and is preferably formed of a material used for a seed film formed on an adhesive film as a sputtering seed layer 73. For example, the processing unit FF1 deposits a copper film using target T2 by sputtering. The ion gun I1 is configured to emit ions onto the substrate S at a desired energy. The processing unit FF1 irradiates, for example, the titanium film deposited using target T1 with ions from the ion gun I1.

[0051] In this embodiment, with the titanium film already formed on the resin layer 6, energy is applied to the titanium film and the resin layer 6 via ion irradiation to form an adhesive layer 7A having a titanium carbide layer 71 made of a titanium carbide bonding layer, and the adhesive layer 7A serves as an excellent adhesive film. When depositing the adhesive layer 7A, the control device CR first rotates the processing unit FF1 so that the target material T1 faces the substrate S, and forms a Ti film on the substrate S using the target material T1 via sputtering. In this state, the control device CR further rotates the processing unit FF1 so that the ion gun I1 faces the substrate S, applies a voltage to the ion gun I1 to emit ions onto the substrate S, and generates plasma from argon gas introduced into the processing chamber 50 through the gas introduction unit G1. Thus, by applying energy to the titanium film and the resin layer 6 formed on the substrate S via ion irradiation, the titanium element contained in the titanium film and the carbon element contained in the resin layer 6 are covalently bonded. Therefore, a titanium carbide layer 71 can be formed from the titanium film. Furthermore, not limited to argon alone, a mixed gas in which nitrogen or an active gas such as oxygen is mixed with argon can be used as the atmosphere gas during ion irradiation by the ion gun I1.

[0052] Next, we will refer to Figures 3 to 4E Further description using Figure 2 The film forming apparatus shown performs a method for manufacturing a laminate according to this embodiment, including a second wiring layer 7. Figure 3 It is shown by Figure 2 The flowchart shows a laminate manufacturing method performed by the film forming apparatus according to this embodiment.

[0053] Figures 4A to 4E This is a cross-sectional view showing the steps of a laminate manufacturing method according to this embodiment, specifically a cross-sectional view showing the steps of a method for manufacturing the wiring portion of a semiconductor package.

[0054] One feature of the laminate manufacturing method according to this embodiment is that when forming Figure 1 When the second wiring layer 7 is shown, energy is applied to the titanium film and the resin layer 6 by ion irradiation while the titanium film has been formed on the resin layer 6, thereby forming a titanium carbide layer 71 from the titanium film.

[0055] like Figure 3 As shown, the laminate manufacturing method according to this embodiment includes a first step (step S102), a second step (step S103), a third step (step S104), and a fourth step (step S105). Furthermore, the laminate manufacturing method according to this embodiment may include an etching step (step S101) preceding the first step (step S102).

[0056] The first step (step S102) is to form a titanium film on the bottom of the resin layer 6 and the via 10. The second step (step S103) is to apply energy to the titanium film formed in the first step (step S102) by ion irradiation after the first step (step S102) to form a titanium carbide layer 71 of the adhesive layer 7A from the titanium film. The third step (step S104) is to form a titanium layer 72 of the adhesive layer 7A after the second step (step S103). The fourth step (step S105) is to form a sputtered seed layer 73 after the third step (step S104). An etching step (step S101) that can be performed before the first step (step S102) is to etch the surface of the substrate S before the first step (step S102) to form the via 10 in the resin layer 6.

[0057] Furthermore, the first step (step S102) and the second step (step S103) can be performed two or more times. By repeating the first step (step S102) and the second step (step S103) two or more times, the bonding ratio of titanium to carbon in the titanium carbide layer 71 from the resin layer 6 side to the titanium layer 72 side can be changed in a gradient manner. That is, the bonding ratio from the resin layer 6 side to the titanium layer 72 side can be gradually reduced. In this way, by changing the bonding ratio between titanium and carbon in the titanium carbide layer 71 in a gradient manner, the adhesion of the titanium carbide layer 71 can be improved.

[0058] exist Figure 2 The above steps are performed on the substrate S shown. Figure 4A As shown, the substrate S is a substrate having a supporting substrate C, a first wiring layer 5 formed on the supporting substrate C by a wiring pattern, for example, through a semi-additive process, and a resin layer 6 formed on the supporting substrate C including the first wiring layer 5. Through-holes 10 reaching the first wiring layer 5 are patterned and formed in the resin layer 6. The supporting substrate C is not particularly limited, but is preferably any one of a silicon (Si) substrate, a glass substrate, and a resin substrate. After this substrate S is introduced into the processing chamber 50 and held by the holding unit 60, the various steps are performed inside the processing chamber 50 as described below.

[0059] First, in the etching step S101, the control device CR rotates the support SP that supports multiple targets T1 and T2 and the ion gun I1 to orient the ion gun I1 toward the substrate S side and make the ion gun I1 face the substrate S. Next, the control device CR introduces argon gas from the gas introduction unit G1 into the processing chamber 50 to stabilize the pressure inside the processing chamber 50, and then applies a voltage to the ion gun I1 to generate plasma from the argon gas. The plasma generated in this way is used to etch the first wiring layer 5 on the supporting substrate C and the resin layer 6 in which the vias 10 are patterned and reach the first wiring layer 5, as shown. Figure 4AAs shown. This etching process cleans the surface of the substrate S. The control device CR stops applying voltage to the ion gun I1 when the etching step S101 is completed.

[0060] Next, in the first step of step S102, the control device CR rotates the support SP that supports multiple targets T1 and T2 and the ion gun I1 to orient the target T1 toward the substrate S side and make the target T1 face the substrate S. Next, after the pressure in the processing chamber 50 stabilizes, the control device CR supplies a preset power to the target T1 to generate plasma from argon gas. The target T1 is sputtered by the plasma generated in this manner, thereby depositing a titanium film P on the resin layer 6 and the first wiring layer 5 exposed at the bottom of the via 10, as shown below. Figure 4B As shown.

[0061] Next, in the second step of step S103, the control device CR rotates the support SP that supports multiple targets T1 and T2 and the ion gun I1 to orient the ion gun I1 toward the substrate S side and make the ion gun I1 face the substrate S. Next, the control device CR introduces argon gas from the gas introduction unit G1 into the processing chamber 50 to stabilize the pressure inside the processing chamber 50, and then applies a voltage to the ion gun I1 to generate plasma from the argon gas. In this way, energy is applied to the titanium film P and the resin layer 6 by ion irradiation by the ion gun I1, thereby modifying the surface of the resin layer 6 of the substrate S, and forming titanium carbide bonding between the titanium elements contained in the titanium film P and the carbon elements contained in the resin layer 6. Therefore, as... Figure 4C As shown, a titanium carbide layer 71 (which is a layer of adhesive layer 7A near resin layer 6) forming part of adhesive layer 7A is formed from titanium film P. At this time, as a result of etching and removing titanium film P by ion irradiation, the first wiring layer 5 is exposed at the bottom of via 10. Note that titanium carbide layer 71 may be partially formed in at least a portion of titanium film P on the resin layer 6 side.

[0062] Next, in the third step of step S104, the control device CR rotates the support SP that supports multiple targets T1 and T2 and the ion gun I1 to orient the target T1 toward the substrate S side and make the target T1 face the substrate S. Next, after the pressure in the processing chamber 50 stabilizes, the control device CR supplies a preset power to the target T1 to generate plasma from argon gas. The plasma generated in this way sputters the target T1, thereby forming a titanium layer 72 on the titanium carbide layer 71, which is the upper layer of the adhesive layer 7A and forms part of the adhesive layer 7A, as shown below. Figure 4D As shown. Titanium layer 72 is formed on the surface of the first wiring layer 5 and on the surface of titanium carbide layer 71.

[0063] Next, in the fourth step of step S105, the control device CR rotates the support member supporting multiple targets T1 and T2 and the ion gun I1 to orient target T2 toward the substrate S side and make target T2 face the substrate S. Next, after the pressure in the processing chamber 50 stabilizes, the control device CR supplies preset power to target T2 to generate plasma from argon gas. The plasma generated in this way sputters target T2, thereby forming a sputtered seed layer 73 on the titanium layer 72 of the adhesive layer 7A, as shown below. Figure 4E As shown. The sputtering seed layer 73 is not particularly limited, but is preferably any one of Cu film, CuAl alloy film, and CuW alloy film. The target material T2 can be appropriately changed according to the type of film to be formed.

[0064] In this way, it is possible to use Figure 2 The film forming apparatus shown forms an adhesive layer 7A and a sputtered seed layer 73 onto a substrate S.

[0065] Until the sputtered seed layer 73 is formed, the substrate S is removed from... Figure 2 The film is removed from the film forming apparatus shown, and the sputtered seed layer 73 can be used as a seed layer to form a copper electroplated layer 74 by electroplating. In this way, a second wiring layer 7 having an adhesive layer 7A, a sputtered seed layer 73, and a copper electroplated layer 74 is formed on the resin layer 6.

[0066] As described above, in this embodiment, the surface of the resin layer 6 is modified by ion irradiation, thereby forming a titanium carbide layer 71 containing titanium elements that form the titanium layer 72 of the adhesive layer 7A between the resin layer 6 and the titanium layer 72. Therefore, the adhesion between the resin layer 6 and the second wiring layer 7, including the sputtered seed layer 73, can be improved. In this embodiment, energy is applied by ion irradiation, thereby inducing unsaturated bonding on the resin layer 6, linking titanium elements with carbon elements in the resin layer 6, and forming a titanium carbide layer 71 between the resin layer 6 and the titanium layer 72. Because the adhesive force between the resin layer 6 and the titanium layer 72 of the adhesive layer 7A is enhanced by this titanium carbide layer 71, the adhesion between the resin layer 6 and the second wiring layer 7 (the adhesive layer 7A, the sputtered seed layer 73, and the copper plating layer 74 are sequentially stacked in the second wiring layer 7) can be ensured.

[0067] As described above, according to this embodiment, since the sputtering seed layer 73 is formed on the resin layer 6 via an adhesive layer 7A having a titanium carbide layer 71 and a titanium layer 72, the adhesion between the resin layer 6 and the sputtering seed layer 73 can be improved.

[0068] Note that the film of resin layer 6, including the first wiring layer 5 and the second wiring layer 7, can be used for manufacturing after being separated from the support substrate C. Figure 1The semiconductor package shown. When manufacturing the semiconductor package, the first wiring layer 5 in the film of resin layer 6 is connected to the wiring 4 of printed wiring substrate 2 by solder 8. Next, an underfill material is filled between the printed wiring substrate 2 and the film of resin layer 6 to form an underfill layer 9.

[0069] [Second Implementation]

[0070] Reference Figure 5 A laminate and a method for manufacturing a laminate according to a second embodiment of the present invention are described. Note that components similar to those in the laminate and the method for manufacturing a laminate in the first embodiment are labeled with the same reference numerals, and their descriptions will be omitted or simplified.

[0071] The difference between this embodiment and the first embodiment is that, by using... Figure 5 The membrane forming apparatus shown is not Figure 2 The film forming apparatus shown is used to form the adhesive layer 7A and the sputtered seed layer 73. Figure 5 This is a cross-sectional view of the film forming apparatus according to this embodiment, taken along a vertical plane. In this document, the XY plane is a plane parallel to the horizontal plane, and the Z-axis is an axis parallel to the vertical direction.

[0072] The basic structure of the membrane forming apparatus according to this embodiment is similar to... Figure 2 The basic structure of the membrane forming apparatus shown is illustrated. Figure 5 As shown, the membrane forming apparatus according to this embodiment and Figure 2 The difference in the film forming apparatus shown is that, in the absence of an ion gun I1, a high-frequency power supply P1 is provided. This high-frequency power supply P1 is configured to apply a high-frequency voltage to the substrate S held by the holding unit 60 via the holding unit 60. As the high-frequency power supply P1, a high-frequency power supply with a variable output voltage can be used. Note that in the film forming apparatus according to this embodiment, an ion gun I1 may also be installed to perform the etching step of step S101.

[0073] In addition to the second step of step S103, using Figure 5 The laminate manufacturing method of the film forming apparatus shown in this embodiment is similar to the laminate manufacturing method according to the first embodiment. The second step of step S103 can also be implemented by applying a high-frequency voltage to the substrate S. In this embodiment, the second step of step S103 is performed by applying a high-frequency voltage to the substrate S using a high-frequency power supply P1, which is a high-frequency voltage application mechanism as described below.

[0074] Specifically, in the second step of step S103, the control device CR rotates the support SP that supports multiple targets T1 and T2, so that the surface of the processing unit FF1 is oriented towards the substrate S side, where no targets T1 and T2 are mounted. Next, the control device CR applies a high-frequency voltage to the substrate S using a high-frequency power supply P1 to generate plasma, attracts ions from the plasma to the substrate S using a self-biased voltage Vdc generated on the substrate S, and applies energy to the titanium film P and resin layer 6 formed in the first step of step S102. This energy application modifies the surface of the resin layer 6 of the substrate S to... Figure 4C The titanium carbide layer 71 (which is the layer of the adhesive layer 7A close to the resin layer 6) is formed in the same manner as the first embodiment shown.

[0075] Similar to this embodiment, the titanium carbide layer 71 can also be formed by applying energy to the titanium film P and the resin layer 6 using ions attracted from a high-frequency power source P1 instead of using an ion gun I1 for ion irradiation.

[0076] [Third Implementation Method]

[0077] Reference Figure 6 A laminate and a method for manufacturing a laminate according to a third embodiment of the present invention are described. Note that components similar to those in the laminates and methods for manufacturing laminates in the first and second embodiments are labeled with the same reference numerals, and their descriptions will be omitted or simplified.

[0078] The difference between this embodiment and the first embodiment is that, by using... Figure 6 The membrane forming apparatus shown is not Figure 2 The film forming apparatus shown is used to form the adhesive layer 7A and the sputtered seed layer 73. Figure 6 This is a cross-sectional view of the film forming apparatus according to this embodiment, taken along a vertical plane. In this document, the XY plane is a plane parallel to the horizontal plane, and the Z-axis is an axis parallel to the vertical direction.

[0079] The basic structure of the membrane forming apparatus according to this embodiment is similar to... Figure 2 The basic structure of the membrane forming apparatus shown is illustrated. Figure 6 As shown, the membrane forming apparatus according to this embodiment and Figure 2 The difference in the film forming apparatus shown is that, without the ion gun I1, a DC power supply P2 is provided. This DC power supply P2 is configured to apply a DC voltage to the substrate S held by the holding unit 60 via the holding unit 60. As the DC power supply P2, a DC power supply with a variable output voltage can be used. Note that in the film forming apparatus according to this embodiment, the ion gun I1 can also be installed to perform the etching step of step S101.

[0080] In addition to the second step of step S103, using Figure 6 The laminate manufacturing method of the film forming apparatus shown in this embodiment is similar to the manufacturing method according to the first embodiment. The second step of step S103 can also be performed by depositing a titanium film while a negative bias voltage is applied to the substrate S. In this embodiment, the second step of step S103 is performed by depositing a titanium film while a negative bias voltage is applied to the substrate S by a DC power supply P2, which is a DC voltage application mechanism as described below.

[0081] Specifically, in the second step of step S103, the control device CR rotates the support SP that supports multiple targets T1 and T2 to orient the target T1 toward the substrate S side and make the target T1 face the substrate S. Next, after the pressure in the processing chamber 50 stabilizes, the control device CR supplies a preset power to the target T1 while applying a negative bias voltage to the substrate S via DC power supply P2 to generate plasma from argon gas. Therefore, while depositing the titanium film by sputtering, energy is applied to the titanium film P and resin layer 6 formed in the first step of step S102 by using a negative bias voltage to attract ions from the plasma to the substrate S. This application of energy modifies the surface of the resin layer 6 on the substrate S to achieve a more uniform appearance. Figure 4C The titanium carbide layer 71 (which is the layer adjacent to the resin layer 6 of the adhesive layer 7A) is formed in the same manner as in the first embodiment shown. In this document, the bias voltage applied to the substrate S by the DC power supply P2 is preferably a DC pulse bias voltage. The negative bias voltage applied to the substrate S can be constant or can be gradually changed over time.

[0082] According to this embodiment, even a film forming apparatus that does not have an ion gun I1 or a high-frequency power supply P1 can form a titanium carbide layer 71.

[0083] [Fourth Implementation Method]

[0084] The laminate and its manufacturing method according to a fourth embodiment of the present invention will now be described. Note that components similar to those in the laminates and their manufacturing methods in the first to third embodiments are labeled with the same reference numerals, and their descriptions will be omitted or simplified.

[0085] The first step of step S102 and the second step of step S103 can also be performed simultaneously. The laminate manufacturing method according to this embodiment uses... Figure 6 The membrane forming apparatus shown below performs the first step of step S102 and the second step of step S103 simultaneously.

[0086] Specifically, while simultaneously executing the first step of step S102 and the second step of step S103, the control device CR rotates the support SP that supports multiple targets T1 and T2 to orient the target T1 toward the substrate S and make the target T1 face the substrate S. Next, after the pressure in the processing chamber 50 stabilizes, the control device CR supplies a preset power to the target T1 while applying a negative bias voltage to the substrate S via a DC power supply P2, to generate plasma from argon gas. Since a titanium film is deposited while energy is applied by ion irradiation using a negative bias voltage, the titanium elements contained in the titanium film are covalently bonded to the carbon elements contained in the resin layer 6. This titanium film deposition under applied energy modifies the surface of the resin layer 6 of the substrate S, thereby achieving a more uniform appearance. Figure 4C The titanium carbide layer 71 (which is the layer adjacent to the resin layer 6 of the adhesive layer 7A) is formed in the same manner as in the first embodiment shown. In this document, the bias voltage applied to the substrate S by the DC power supply P2 is preferably a DC pulse bias voltage. The negative bias voltage applied to the substrate S can be constant or can be gradually changed over time.

[0087] According to this embodiment, by simultaneously executing the first step of step S102 and the second step of step S103, productivity can be improved, and even a film forming device that does not have an ion gun I1 or a high-frequency power supply P1 can form a titanium carbide layer 71.

[0088] The following will refer to Figures 7 to 9 Examples of the present invention are described below.

[0089] The bonding state of the interface between the resin layer and the adhesive film was measured using an X-ray photoelectron spectroscopy (SSX-100, from Surface Science Instruments). The measurement was performed non-destructively, using an AlKα (1487 eV) X-ray source configured such that the angle between the sample stage and the analyzer was 90 degrees to maximize the detection depth of the photoelectrons. The measurement was performed until... Figure 3 The second step of step S103 in the film formation process shown is used to produce a measurement sample, that is, the etching step of step S101, the first step of step S102, and the second step of step S103 in the method according to the first embodiment are performed. In the first step of step S102, a titanium film of 3 nm is deposited. In addition, a sample on which the second step of step S103 is not performed is produced for comparison. Note that since the photoelectrons generated in X-ray photoelectron spectroscopy are subjected to inelastic scattering inside the sample, the interface between the resin layer and the adhesive film cannot be analyzed when the titanium film is thick. Therefore, the sample is produced in a way that makes the titanium film thickness 10 nm or less.

[0090] Figure 7This is a diagram showing an example of a C1s spectrum obtained by X-ray photoelectron spectroscopy measurement, and Figure 8 This is a diagram showing an example of a Ti2p spectrum. Figure 7 and Figure 8 The horizontal axis represents the measured binding energy of the electron to the atomic nucleus, and its vertical axis represents the intensity of the emitted photoelectrons. Figure 7 and Figure 8 In the diagram, solid-line spectra represent examples of measurement results for samples on which the second step up to step S103 has been performed, while dashed-line spectra represent examples of measurement results for comparison samples on which the second step S103 has not been performed. Elements have different binding energies depending on their binding state with neighboring atoms. Therefore, information about the binding state can be obtained from the binding energy.

[0091] First, in relation to Figure 7 When comparing the C1s spectra shown, a peak was detected near 282.0 eV for the measurement sample in which ion irradiation was performed on the titanium film on the resin layer formed in the first step in the second step, which was not observed in the comparison sample without ion irradiation. Next, in comparison with... Figure 8 When comparing the Ti2p spectra shown, a peak was detected near 455.0 eV for the measurement sample in which ion irradiation was performed on the titanium film on the resin layer formed in the first step in the second step, which was not observed in the comparison sample without ion irradiation.

[0092] Figure 7 The peak value of the C1s spectrum near 282.0 eV and Figure 8 The peaks near 455.0 eV in the Ti2p spectrum are due to titanium carbide bonding, where carbon and titanium are linked. Figure 7 and Figure 8 The measurement results showed a peak in bonding energy due to titanium carbide bonding, confirming the formation of titanium carbide bonding.

[0093] Next, Table 1 shows the results of checking whether titanium carbide bonding was formed for each film thickness and each ion irradiation time when the titanium film on the resin layer was subjected to ion irradiation according to the scheme of the first embodiment. The formation of titanium carbide bonding was confirmed by X-ray photoelectron spectroscopy.

[0094] [Table 1]

[0095]

[0096]

[0097] As shown in Table 1, the results obtained indicate that no titanium carbide bonds are formed when ion irradiation is not performed after titanium film deposition. Conversely, titanium carbide bonds are formed when ion irradiation is performed on the titanium film on the resin layer formed in the first step. Furthermore, when the titanium film thickness is 2.5 nm or greater, it has been confirmed that titanium carbide bonds are formed during ion irradiation.

[0098] Next, Table 2 shows the results of checking whether titanium carbide bonding was formed for various ion energies when a titanium thin film with a thickness of 5 nm formed on the resin layer was subjected to ion irradiation according to the scheme of the first embodiment.

[0099] [Table 2]

[0100]

[0101] As shown in Table 2, the result obtained is that titanium carbide bonding was formed by performing ion irradiation on the titanium film on the resin layer.

[0102] Next, Figure 9 The results of the peel strength measurements for the laminates obtained in Examples 1 to 4 and the laminates obtained in the comparative examples are shown. Figure 9 This is a graph showing the peel strength measured for the laminates obtained in Examples 1 to 4 and the laminates obtained in the comparative example.

[0103] The laminate obtained in Example 1 is the laminate obtained in the first embodiment. The laminate obtained in Example 2 is the laminate obtained in the second embodiment. The laminate obtained in Example 3 is the laminate obtained in the third embodiment. The laminate obtained in Example 4 is the laminate obtained in the fourth embodiment. In each example, a photosensitive polyimide resin layer is used as resin layer 6.

[0104] Except for omitting the first step of step S102 and the second step of step S103, the laminate obtained in the comparative example is similar to the laminate obtained in Example 1. In the comparative example, instead of performing the first step of step S102 and the second step of step S103, the titanium carbide layer is formed by sputtering a titanium carbide target under an argon atmosphere before the third step of step S104.

[0105] In the peel strength measurement, a 90-degree peel test was performed using a peel testing machine (Shimadzu Autograph AG-100kNXplus). In the 90-degree peel test, the peel strength was measured when the second wiring layer 7, in which the adhesive layer 7A, the sputtered seed layer 73, and the copper plating layer 74 are sequentially stacked, peeled off from the resin layer 6. Note that the 90-degree peel test was conducted at a test chamber temperature of 23±2℃ and a test chamber humidity of 50±5%RH, and the test rate was 10 mm / min. Figure 9 The normalized peel strength of the laminates obtained in Examples 1 to 4 and the comparative example is shown.

[0106] like Figure 9 As shown, the peel strength measured for the laminates of Examples 1 to 4 was found to be 1.35 to 1.5 times that measured for the laminates of the comparative examples. It has been confirmed that the adhesion between the resin layer (as an interlayer insulating film) and the seed layer can be improved by applying the present invention.

[0107] [Variant Implementation]

[0108] Although preferred first to fourth embodiments of the present invention have been described above, the present invention is not limited to these first to fourth embodiments, and various modifications and alterations can be made within its spirit.

[0109] For example, although the case where the adhesive layer 7A is a Ti-containing layer has been described as an example in the first to fourth embodiments described above, the adhesive layer 7A is not limited to a Ti-containing layer. As the adhesive layer 7A, for example, a layer containing Ta, Ni, Cr, TiN, Ti alloy, Ta alloy, Ni alloy, Cr alloy, etc., can be used as the adhesive film between the Cu seed layer and a resin layer such as an interlayer insulating film. In this case, the adhesive layer 7A can be a laminate having a metal carbide layer on the resin layer 6 side, such as: TaC layer and Ta layer; NiC layer and Ni layer; CrC layer and Cr layer; TiNC layer and TiN layer; Ti alloy-C layer and Ti alloy layer; Ta alloy-C layer and Ta alloy layer; Ni alloy-C layer and Ni alloy layer; Cr alloy-C layer and Cr alloy layer, etc. The metal carbide layer can be formed in the same manner as the titanium carbide layer 71 according to each of the first to fourth embodiments described above.

[0110] Furthermore, although the case where the sputtering seed layer 73 is a Cu layer has been described as an example in the first to fourth embodiments described above, the sputtering seed layer 73 is not limited to a Cu layer. For example, an alloy layer containing Cu (such as a CuAl alloy layer, a CuW alloy layer, etc.) may also be used as the sputtering seed layer 73.

[0111] Furthermore, although the resin layer 6 has been described as an insulating resin layer serving as an interlayer insulating film in the wiring portion 1 of a semiconductor package as an example in the first to fourth embodiments described above, the resin layer 6 is not limited to serving as an insulating resin layer serving as an interlayer insulating film in the wiring portion 1 of a semiconductor package. For example, the resin layer 6 can be a resin substrate serving as a printed circuit board, specifically, it can be a glass epoxy board, a fluoropolymer substrate, a polyimide film, etc. In this case, the laminate can be a laminate having a resin substrate serving as the resin layer 6, an adhesive layer 7A, and a sputtering seed layer 73 in sequence.

Claims

1. A method for manufacturing a laminate, comprising: The etching step etches the first wiring layer and the resin layer having vias extending to the first wiring layer. The first step involves forming a titanium film on the resin layer and the first wiring layer; The second step following the first step involves removing the titanium film by applying energy to it, while simultaneously forming a titanium carbide layer on the resin layer that forms part of the adhesive layer. A third step following the second step involves forming a titanium layer on the first wiring layer exposed by the removal of the titanium film, and forming a titanium layer constituting part of the adhesive layer on the titanium carbide layer; and The fourth step following the third step involves forming a seed crystal layer on the titanium layer. The titanium carbide layer is formed by applying energy to a titanium film already formed on the resin layer, causing the titanium elements in the titanium film to covalently bond with the carbon elements in the resin layer. In the second step, applying energy to the titanium film is at least one of the following: Ion irradiation, A high-frequency voltage is applied to a substrate having the resin layer and the first wiring layer to generate plasma, attracting ions through a self-biased voltage generated on the substrate, and A negative bias voltage is applied to a substrate on which the resin layer and the first wiring layer are formed, and ions are attracted by the negative bias voltage.

2. The method for manufacturing a laminate according to claim 1, wherein, The second step involves applying the energy to the titanium film to modify the surface of the resin layer and forming the titanium carbide layer on at least the portion of the titanium film located on the side of the resin layer.

3. The method for manufacturing a laminate according to claim 1, wherein, The titanium carbide layer is formed by repeating the first step and the second step more than twice. The titanium carbide layer is a layer in which the ratio of titanium to carbon in the titanium carbide layer changes in a gradient manner from the resin layer side to the titanium layer side.

4. The method for manufacturing a laminate according to claim 1, wherein, The resin layer is formed from a cured resin, which is a polyimide-based resin, an epoxy-based resin, a phenol-based resin, or a polybenzoxazole-based resin.

Citation Information

Patent Citations

  • Semiconductor device and method for manufacturing the same

    WO2008105535A1

  • Semiconductor device having an adhesion layer

    US6720659B1