A method for preparing ultrafine carbon nanotube catalyst

By using a hydrothermal synthesis method controlled by multiple vertical pipe bodies and hydraulic cylinders in the hydrothermal reactor, the problems of catalyst particles agglomeration and small yield are solved, and the preparation of ultrafine carbon nanotube catalyst with uniform particle size is achieved, improving the Catalyst performance and efficiency of industrial applications.

CN115999648BActive Publication Date: 2024-11-01JIAOZUO JIYUE NANO MATERIAL TECH CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202211232267.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-10
Publication Date
2024-11-01
Estimated Expiration
2042-10-10

AI Technical Summary

Technical Problem

In the prior art, the preparation method of carbon nanotube catalysts is easy to agglomerate, resulting in large particle size and uneven distribution. In industrial preparation, hydrothermal synthesis method has small single yield, low efficiency and high heating and cooling consumption. and the problem of high sealing requirements.

Method used

Hydrothermal synthesis is performed using a hydrothermal reactor with multiple vertical pipe bodies. The reaction pressure and temperature are controlled by the hydraulic cylinder to achieve the preparation of ultrafine carbon nanotube catalyst with uniform particle size, reduce the temperature difference and concentration difference, and improve the reaction conditions. Control the accuracy and optimize the reaction process through preheating and cooling mechanisms.

Benefits of technology

Ultrafine powder with uniform particle size was successfully prepared to obtain high-quality carbon nanotubes with small tube diameters, which improved the performance and yield of the catalyst, and reduced the energy consumption of the reaction process and the deformation risk of equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115999648B_ABST
    Figure CN115999648B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing an ultrafine carbon nanotube catalyst, comprising the following steps: 1) dissolving a metal salt in water to prepare a solution A; dissolving ammonium carbonate in water to prepare a solution B; 2) mixing the solution A and the solution B to obtain a suspension precursor, transferring the suspension precursor into a hydrothermal reactor for hydrothermal reaction, cooling, and drying the residual liquid to obtain a catalyst. The present invention adopts a hydrothermal synthesis method to prepare a carbon nanotube catalyst, and can obtain an ultrafine powder with uniform particle size, which is conducive to the preparation of high-quality carbon nanotubes with small diameters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an ultrafine carbon nanotube catalyst, belonging to the technical field of carbon nanotube preparation. Background Art

[0002] The conductive agents commonly used in lithium-ion batteries currently include carbon black, conductive graphite, VGCF, carbon nanotubes and graphene, etc. Among them, carbon black, conductive graphite and VGCF are traditional conductive agents; carbon nanotubes and graphene are new conductive agent materials.

[0003] Carbon nanotubes can be divided into two categories: single-walled tubes and multi-walled tubes. One-dimensional carbon nanotubes are cylindrical, hollow inside, and have good electronic conductivity. The fiber structure can make point-to-line contact with the active material, forming a continuous conductive network in the electrode active material, acting as a "wire", which is beneficial to improving battery capacity, rate performance, battery cycle life, and reducing battery interface impedance. Under the same conductive effect, the amount of carbon nanotubes used is only 1 / 6-1 / 2 of traditional carbon black, which can greatly improve the energy density of lithium batteries. At present, the industry generally uses chemical vapor deposition (CVD) to manufacture carbon nanotubes. This method has a low temperature and is easy to control, with high product yield and carbon purity. The finer the diameter of the carbon nanotube, the longer the length, the higher the heat exchange performance along the length direction, and the higher the carbon purity, the better the conductivity. The catalyst is the key to determining the diameter and purity of the carbon nanotube. The finer the catalyst particles, the smaller the diameter of the grown carbon nanotubes. In the prior art, the catalyst is generally prepared by coprecipitation method, and the precipitate obtained by filtration needs to be calcined and ball-milled. The disadvantage is that the obtained catalyst particles are easy to agglomerate, resulting in a larger particle size of the catalyst particles and uneven particle size distribution. In addition, there is a hydrothermal synthesis method that can directly obtain nano-scale catalyst particles, and the particles are not agglomerated and the particle size distribution is uniform. However, this method only exists in the laboratory for small-dose preparation, and the single-time output is at the milligram level, and it cannot be applied to the industrial preparation of catalysts at present. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for preparing an ultrafine carbon nanotube catalyst, the specific scheme is as follows:

[0005] A method for preparing an ultrafine carbon nanotube catalyst comprises the following steps:

[0006] 1) Dissolve the metal salt in water to prepare solution A; dissolve ammonium carbonate in water to prepare solution B;

[0007] 2) Solution A and solution B are mixed to obtain a suspension precursor, and the suspension precursor is transferred into a hydrothermal reactor for hydrothermal reaction. After cooling, the residual liquid is dried to obtain a catalyst.

[0008] Furthermore, the metal salt includes one or more of the hydrochloride, nitrate or sulfate of iron, cobalt or nickel.

[0009] Furthermore, the metal salt also includes one or more of aluminum and magnesium hydrochlorides, nitrates or sulfates.

[0010] Furthermore, the hydrothermal reactor includes a vertically arranged cylinder, an upper plug is provided on the upper part of the cylinder, and a lower plug is provided on the lower part, and the upper plug and the lower plug are both slidably and sealedly connected to the inner wall of the cylinder; the upper plug and the lower plug are both provided with a vertical hydraulic cylinder; an upper partition and a lower partition are provided in the cylinder, and a heating chamber is provided between the upper partition and the lower partition, and the heating chamber is provided with an inlet and outlet for heat transfer oil; a plurality of vertical pipe bodies are also provided in the cylinder, and the pipe bodies pass through the upper partition and the lower partition, and the pipe bodies are slidably and sealedly connected to the upper partition and the lower partition; a feed inlet is provided on the cylinder along the upper part of the upper partition, and a discharge outlet is provided along the lower part of the lower partition; overflow ports are provided at both ends of the pipe body.

[0011] Furthermore, both ends of the tube body are closed, and the overflow port is arranged on the side wall of the tube body and close to the end of the tube body.

[0012] Furthermore, the height of the heating chamber is 1 / 2-2 / 3 of the length of the tube body.

[0013] Furthermore, a preheating mechanism is provided on the outer wall of the cylinder along the upper part of the upper partition, and a cooling mechanism is provided along the lower part of the lower partition.

[0014] Furthermore, a gas phase balance port is provided on the side wall of the cylinder along the lower part of the lower partition, the gas phase balance port is located at the top, and the discharge port is located at the bottom.

[0015] Furthermore, the operation steps of the hydrothermal reactor include:

[0016] 1) The hydraulic cylinder drives the upper plug and the lower plug to move upward to the upper limit first, the gas phase balance port and the discharge port are closed, the feed port is opened, and the suspension precursor is injected, and the suspension precursor fills the tube body;

[0017] 2) The feed port is closed, and heat transfer oil is injected into the heating chamber for heating, and the temperature is kept constant until the reaction is completed:

[0018] 3) The hydraulic cylinder drives the upper plug and the lower plug to move downward to the lower limit position, and the mixed liquid in the tube body enters under the lower partition. After cooling, the gas phase balance port and the discharge port are opened, and the residual liquid is discharged along the discharge port.

[0019] The present invention adopts a hydrothermal synthesis method to prepare a carbon nanotube catalyst, and can obtain ultrafine powder with uniform particle size, which is beneficial to the preparation of high-quality carbon nanotubes with small tube diameters.

[0020] The volume of the hydrothermal reactor used for hydrothermal synthesis in the laboratory is generally 50 / 100 / 250ml, and the filling rate is generally controlled at 60-80%, and the single output is only tens of milligrams. Moreover, hydrothermal synthesis is greatly affected by conditions such as pressure and temperature. When the conditions change, the reaction may not be carried out and the expected product cannot be obtained. Even under laboratory conditions, using a small-volume reactor, there is often no precipitation after the reaction, or the precipitate is in a gel state. When the volume of the reaction vessel is expanded, the kinetic conditions change greatly, and the problem of uneven temperature and concentration in various parts of the system is amplified, making it more difficult to achieve smooth hydrothermal synthesis.

[0021] In addition, hydrothermal synthesis needs to be carried out under high pressure conditions, which places high demands on container sealing. The reactor adopts an intermittent working mode. After each reaction is completed, the reactor body needs to be cooled, emptied, reloaded and sealed, and heated. Firstly, the efficiency is low, and secondly, the alternating heating and cooling consumes high energy. The reactor body is large in size and easy to deform.

[0022] The present invention designs a hydrothermal reactor, which uses multiple tubes for hydrothermal reaction. The volume of a single tube is small, which can reduce the temperature difference and concentration difference, and is conducive to the control of hydrothermal reaction conditions. The material is put in and out by lifting the tube, which has little effect on the sealing conditions of the reactor, and the reaction pressure can be easily controlled by the hydraulic cylinder. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a structural schematic diagram of the hydrothermal reaction kettle in the present invention;

[0024] Figure 2 It is a schematic diagram of the structure of the tube body in the present invention. DETAILED DESCRIPTION

[0025] Example 1

[0026] A method for preparing an ultrafine carbon nanotube catalyst comprises the following steps:

[0027] 1) Dissolve the metal salt in water to prepare solution A; dissolve ammonium carbonate in water to prepare solution B;

[0028] 2) Solution A and solution B are mixed to obtain a suspension precursor, and the suspension precursor is transferred into a hydrothermal reactor for hydrothermal reaction. After cooling, the residual liquid is dried to obtain a catalyst.

[0029] The metal salt includes one or more of the hydrochloride, nitrate or sulfate of iron, cobalt or nickel.

[0030] It also includes one or more of the hydrochlorides, nitrates or sulfates of aluminum and magnesium.

[0031] The ratio of solution A to solution B is set according to the ratio of the metal salt to completely generate a precipitate. The hydrothermal reaction is carried out under conventional conditions, such as a heating temperature of about 250°C, a pressure of 3 to 6 MPa, and a heat preservation time of 8 to 16 hours.

[0032] like Figure 1 and Figure 2 The hydrothermal reactor comprises a vertically arranged cylinder 1, which is made of a pressure-resistant stainless steel structure with a wall thickness of more than 2 cm; an upper plug 2 is provided at the upper part of the cylinder, and a lower plug 3 is provided at the lower part, and both the upper plug and the lower plug are slidably sealed and connected to the inner wall of the cylinder, and a polytetrafluoroethylene sealing ring is provided at the sliding connection; both the upper plug and the lower plug are provided with a vertical hydraulic cylinder 4, and the hydraulic cylinder is used to push the upper plug and the lower plug to move up and down while maintaining the high pressure conditions during the reaction; an upper baffle 5 and a lower baffle are provided in the cylinder. 6. A heating chamber is provided between the upper partition and the lower partition, and a heat transfer oil inlet and outlet 7 is provided in the heating chamber, and the heat transfer oil is used to heat the heating chamber; a plurality of vertical pipe bodies 8 are also provided in the cylinder body, and the pipe bodies penetrate the upper partition and the lower partition, and the pipe bodies are connected with the upper partition and the lower partition in a sliding and sealing manner, and polytetrafluoroethylene sealing rings are also provided along the sliding connection between the upper partition and the lower partition; a feed inlet 9 is provided on the cylinder body along the upper side of the upper partition, and a discharge outlet 10 is provided along the lower side of the lower partition; overflow ports 11 are provided at both ends of the pipe body.

[0033] A polytetrafluoroethylene lining is arranged inside the tube body, and the tube body is used as a reaction space for hydrothermal reaction. The tube diameter is set at 50-100 mm. The heat transfer oil in the heating chamber can directly heat each tube body, and the temperature difference inside the tube body is small. The volume of a single tube body is small, and the kinetic conditions are easy to control during the reaction process.

[0034] The upper and lower partitions are also made of 2 cm thick stainless steel plates.

[0035] In this embodiment, both ends of the tube body are closed, and the overflow port is arranged on the side wall of the tube body and close to the end of the tube body.

[0036] Taking the upper baffle as an example, after the upper plug descends to the lower limit, the end of the tube body sinks below the upper surface of the upper baffle, and the upper baffle can form a seal for the overflow port. When the thickness of the upper baffle is not enough to form a seal for the overflow port, a sleeve can be set on the lower surface of the upper baffle. For example, the overflow port can be set as a strip port. When the length of the strip port is 3 cm, a sleeve with a height of 2 to 4 cm can be set on the lower surface of the upper baffle to ensure that the overflow port is sealed. The lower baffle can adopt the same structure. The upper baffle and the lower baffle are fixedly and sealedly connected to the inner wall of the cylinder.

[0037] The height of the heating chamber is 1 / 2-2 / 3 of the length of the tube. The height of the heating chamber must ensure that there is enough heating space for a single reaction. When the heating chamber is filled with heat transfer oil, it can support the upper and lower partitions to prevent deformation of the upper and lower partitions.

[0038] In this embodiment, a preheating mechanism is provided on the outer wall of the cylinder along the upper side of the upper partition, and a cooling mechanism is provided along the lower side of the lower partition. The preheating mechanism may adopt an electric heating jacket to heat the upper part of the cylinder. The cooling mechanism may adopt a water cooling jacket to cool the material entering below the lower partition.

[0039] In this embodiment, a gas phase balance port 12 is provided on the side wall of the cylinder along the lower part of the lower partition, the gas phase balance port is located at the top, and the discharge port is located at the bottom. The gas phase balance port is used to achieve gas phase balance in the space below the lower partition.

[0040] The operation steps of the hydrothermal reactor include:

[0041] 1) The hydraulic cylinder drives the upper plug and the lower plug to move upward to the upper limit first, the gas phase balance port and the discharge port are closed, the feed port is opened, and the suspension precursor is injected, and the suspension precursor fills the tube body;

[0042] 2) The feed port is closed, and heat transfer oil is injected into the heating chamber for heating, and the temperature is kept constant until the reaction is completed:

[0043] 3) The hydraulic cylinder drives the upper plug and the lower plug to move downward to the lower limit position, and the mixed liquid in the tube body enters under the lower partition. After cooling, the gas phase balance port and the discharge port are opened, and the residual liquid is discharged along the discharge port.

Claims

1. A method for preparing an ultrafine carbon nanotube catalyst, characterized in that: The following steps are involved: 1) Dissolve the metal salt in water to prepare solution A; dissolve ammonium carbonate in water to prepare solution B; 2) Solution A and solution B are mixed to obtain a suspension precursor, which is transferred into a hydrothermal reactor for hydrothermal reaction. After cooling, the residual liquid is dried to obtain a catalyst; The hydrothermal reactor comprises a vertically arranged cylinder, an upper plug is provided at the upper part of the cylinder, and a lower plug is provided at the lower part, and both the upper plug and the lower plug are slidably and sealedly connected to the inner wall of the cylinder; both the upper plug and the lower plug are provided with a vertical hydraulic cylinder; an upper baffle and a lower baffle are provided in the cylinder, a heating chamber is provided between the upper baffle and the lower baffle, and a heat transfer oil inlet and outlet are provided in the heating chamber; a plurality of vertical pipe bodies are also provided in the cylinder, the pipe bodies penetrate the upper baffle and the lower baffle, and the pipe bodies are slidably and sealedly connected to the upper baffle and the lower baffle; a feed port is provided along the upper part of the cylinder, and a discharge port is provided along the lower part of the lower baffle; overflow ports are provided at both ends of the pipe body; Both ends of the tube body are closed, and the overflow port is arranged on the side wall of the tube body and close to the end of the tube body; A preheating mechanism is provided on the outer wall of the cylinder along the upper part of the upper partition; The side wall of the cylinder is provided with a gas phase balance port along the lower side of the lower partition; The operation steps of the hydrothermal reactor include: 1) The hydraulic cylinder drives the upper plug and the lower plug to move upward to the upper limit first, the gas phase balance port and the discharge port are closed, the feed port is opened, and the suspension precursor is injected, and the suspension precursor fills the tube body; 2) The feed port is closed, and heat transfer oil is injected into the heating chamber for heating, and the temperature is kept constant until the reaction is completed: 3) The hydraulic cylinder drives the upper plug and the lower plug to move downward to the lower limit position, and the mixed liquid in the tube body enters under the lower partition. After cooling, the gas phase balance port and the discharge port are opened, and the residual liquid is discharged along the discharge port.

2. The method for preparing an ultrafine carbon nanotube catalyst according to claim 1, characterized in that: The metal salt includes one or more of the hydrochloride, nitrate or sulfate of iron, cobalt or nickel.

3. The method for preparing the ultrafine carbon nanotube catalyst according to claim 2, characterized in that: The metal salt also includes one or more of aluminum and magnesium hydrochlorides, nitrates or sulfates.

4. The method for preparing ultrafine carbon nanotube catalyst according to claim 1, characterized in that: The height of the heating chamber is 1 / 2-2 / 3 of the length of the tube body.

5. The method for preparing ultrafine carbon nanotube catalyst according to claim 4, characterized in that: A cooling mechanism is provided along the lower side of the lower partition.

Citation Information

Patent Citations

  • Catalytic reaction equipment

    CN102160981A

  • Carbon doped nano tube aerogel and preparation method and application thereof

    CN104437279A

  • Solid-phase atmosphere reaction device

    CN105032306A

  • Catalyst produced by using hydrothermal synthesis coprecipitation technique, and carbon nanotube manufactured by using same

    CN106132537A

  • Reaction system for preparing carbon materials

    CN109261100A