A rubber mixing method in an internal mixer
By adding liquid polybutene in batches to the internal mixer and maintaining the pressure, the problem of long rubber dissolution time in the rubber industry is solved, and the effects of shortening the dissolution time and reducing energy consumption are achieved.
Patent Information
- Application Number
- CN202211517786.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-30
AI Technical Summary
In the rubber industry, the rubber dissolution time is long during the production process of rat glue, and the crushing operation is difficult. It is difficult to effectively shorten the dissolution time with existing technology.
Butyl rubber and liquid polybutene are mixed in an internal mixer according to a specific mass ratio. By adding liquid polybutene in batches and maintaining the pressure of the internal mixer, the dissolution time is shortened. Specific steps include adding butyl rubber to an internal mixer for internal mixing, adding liquid polybutene at intervals, performing internal mixing for 6 to 10 minutes under a pressure of 0.2 to 0.6 MPa, and finally cutting into long strips.
This method significantly shortens the dissolution time of the rubber, thereby reducing the energy consumption and time of the entire preparation process.
Smart Images

Figure BDA0003972457210000051 
Figure BDA0003972457210000061 
Figure BDA0003972457210000062
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of internal mixing, and in particular to a rubber internal mixing method in an internal mixer. Background Art
[0002] Internal mixers have been used in the rubber industry for a hundred years. The emergence of internal mixers is an important achievement of rubber mixing machinery. It is still a typical equipment in plasticizing and mixing, and is in continuous development and improvement.
[0003] In the current production process of mouse glue, the rubber takes a long time to dissolve. In order to shorten the dissolution time, the rubber is usually crushed, and the smaller the crushed pieces, the better. However, the rubber crushing operation is difficult, and even after crushing, the dissolution time is still relatively long. Summary of the invention
[0004] To solve the above technical problems, the object of the present invention is to provide a rubber mixing method in an internal mixer.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] A rubber mixing method in an internal mixer comprises the following steps:
[0007] Step 1: Add all the butyl rubber into an internal mixer, and mix them in the internal mixer for 6 to 10 minutes at a pressure of 0.2 to 0.6 MPa;
[0008] Step 2: Add liquid polybutene to the internal mixer in 2 to 5 equal portions, with an interval of 5 to 10 minutes between each portion, and keep the internal mixer pressure at 0.2 to 0.6 MPa during the internal mixer;
[0009] Step 3: After the mixing is completed, discharge the material, let it cool, and then cut it into strips of 30-40cm*4-7cm.
[0010] Preferably, in the rubber mixing method in an internal mixer, the mass proportion of the butyl rubber and the liquid polybutene is as follows:
[0011] Butyl rubber: 100 parts;
[0012] Liquid polybutene: 15-25 parts.
[0013] Preferably, the rubber mixing method in an internal mixer comprises mixing the rubber in a mass ratio of 100 parts of butyl rubber and 21 parts of liquid polybutene.
[0014] The following steps are involved:
[0015] (1) Add all the butyl rubber into an internal mixer and mix for 6 minutes at a pressure of 0.4 MPa;
[0016] (2) adding 7 parts by mass of liquid polybutene and kneading for 5 minutes at a pressure of 0.4 MPa;
[0017] (3) adding 7 parts by mass of liquid polybutene and continuing kneading for 5 minutes at a pressure of 0.4 MPa;
[0018] (4) 7 parts by mass of liquid polybutene was added, and the mixture was further kneaded for 5 minutes under a pressure of 0.4 MPa, and then the mixture was discharged.
[0019] (5) Cut the kneaded rubber into strips of 30 cm*4 cm.
[0020] Preferably, the rubber mixing method in an internal mixer comprises mixing the rubber in a mass ratio of 100 parts of butyl rubber and 25 parts of liquid polybutene.
[0021] The following steps are involved:
[0022] (1) Add all the butyl rubber into an internal mixer and mix for 10 minutes at a pressure of 0.4 MPa;
[0023] (2) adding 5 parts by mass of liquid polybutene and kneading for 7 minutes at a pressure of 0.3 MPa;
[0024] (3) adding 5 parts by mass of liquid polybutene and continuing kneading for 7 minutes at a pressure of 0.3 MPa;
[0025] (4) 5 parts by mass of liquid polybutene were added, and kneading was continued for 7 minutes at a pressure of 0.3 MPa.
[0026] (5) 5 parts by mass of liquid polybutene were added, and kneading was continued for 7 minutes at a pressure of 0.3 MPa.
[0027] (6) Add 5 parts by mass of liquid polybutene, continue kneading for 7 minutes at a pressure of 0.3 MPa, and discharge the mixture.
[0028] (7) Cut the kneaded rubber into strips of 35 cm*5 cm.
[0029] Preferably, the rubber mixing method in the internal mixer is mixing the rubber in a ratio of 100 parts by weight of butyl rubber and 16 parts by weight of liquid polybutene.
[0030] The following steps are involved:
[0031] (1) Add all the butyl rubber into an internal mixer and mix for 8 minutes at a pressure of 0.4 MPa.
[0032] (2) adding 8 parts by mass of liquid polybutene and kneading for 10 minutes at a pressure of 0.6 MPa;
[0033] (3) 8 parts by mass of liquid polybutene were added, and the mixture was further kneaded for 10 minutes under a pressure of 0.6 MPa, and then the mixture was discharged.
[0034] (4) Cut the kneaded rubber into strips of 35 cm*6 cm.
[0035] Preferably, the rubber mixing method in the internal mixer is mixing the rubber in a ratio of 100 parts by weight of butyl rubber and 24 parts by weight of liquid polybutene.
[0036] The following steps are involved:
[0037] (1) Add all the butyl rubber into an internal mixer and mix for 8 minutes at a pressure of 0.4 MPa.
[0038] (2) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa;
[0039] (3) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa;
[0040] (4) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa;
[0041] (5) 6 parts by mass of liquid polybutene were added, and the mixture was further kneaded for 8 minutes under a pressure of 0.5 MPa, and then the mixture was discharged.
[0042] (6) Cut the kneaded rubber into strips of 38 cm*7 cm.
[0043] By means of the above scheme, the present invention has at least the following advantages:
[0044] The invention can shorten the dissolution time, thereby shortening the time of the entire preparation process of the mouse glue, and further reducing energy consumption.
[0045] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0047] Therefore, the following detailed description of the embodiments in the present application is not intended to limit the scope of the present application for protection, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0048] Example
[0049] A rubber mixing method in an internal mixer comprises the following steps:
[0050] Step 1: Add all the butyl rubber into an internal mixer, and mix them in the internal mixer for 6 to 10 minutes at a pressure of 0.2 to 0.6 MPa;
[0051] Step 2: Add liquid polybutene to the internal mixer in 2 to 5 equal portions, with an interval of 5 to 10 minutes between each portion, and keep the internal mixer pressure at 0.2 to 0.6 MPa during the internal mixer;
[0052] Step 3: After the mixing is completed, discharge the material, let it cool, and then cut it into strips of 30-40cm*4-7cm.
[0053] The mass proportion of the butyl rubber and the liquid polybutene in the present invention is as follows:
[0054] Butyl rubber: 100 parts;
[0055] Liquid polybutene: 15-25 parts.
[0056] Embodiment 1
[0057] Based on the above-mentioned embodiment, a rubber mixing method in an internal mixer is provided, wherein the mixing ratio by mass of butyl rubber: 100 parts and liquid polybutene: 21 parts is used for mixing.
[0058] The following steps are involved:
[0059] (1) Add all the butyl rubber into an internal mixer and mix for 6 minutes at a pressure of 0.4 MPa;
[0060] (2) adding 7 parts by mass of liquid polybutene and kneading for 5 minutes at a pressure of 0.4 MPa;
[0061] (3) adding 7 parts by mass of liquid polybutene and continuing kneading for 5 minutes at a pressure of 0.4 MPa;
[0062] (4) 7 parts by mass of liquid polybutene was added, and the mixture was further kneaded for 5 minutes under a pressure of 0.4 MPa, and then the mixture was discharged.
[0063] (5) Cut the kneaded rubber into strips of 30 cm*4 cm.
[0064] Table 1
[0065]
[0066] From Experiment A and Experiment B in Table 1 above, it can be known that the rubber after mixing can improve the efficiency of dissolution, thereby shortening the preparation time of mouse glue.
[0067] Embodiment 2
[0068] Based on the above embodiment, a rubber mixing method in an internal mixer is provided, wherein the mixing ratio by mass of butyl rubber: 100 parts and liquid polybutene: 25 parts is used for mixing.
[0069] The following steps are involved:
[0070] (1) Add all the butyl rubber into an internal mixer and mix for 10 minutes at a pressure of 0.4 MPa;
[0071] (2) adding 5 parts by mass of liquid polybutene and kneading for 7 minutes at a pressure of 0.3 MPa;
[0072] (3) adding 5 parts by mass of liquid polybutene and continuing kneading for 7 minutes at a pressure of 0.3 MPa;
[0073] (4) 5 parts by mass of liquid polybutene were added, and kneading was continued for 7 minutes at a pressure of 0.3 MPa.
[0074] (5) 5 parts by mass of liquid polybutene were added, and kneading was continued for 7 minutes at a pressure of 0.3 MPa.
[0075] (6) Add 5 parts by mass of liquid polybutene, continue kneading for 7 minutes at a pressure of 0.3 MPa, and discharge the mixture.
[0076] (7) Cut the kneaded rubber into strips of 35 cm*5 cm.
[0077] Table 2
[0078]
[0079] From Experiment A and Experiment B in Table 2 above, it can be known that the rubber after mixing can improve the dissolution efficiency, thereby shortening the preparation time of mouse glue.
[0080] Embodiment 3
[0081] Based on the above embodiment, a rubber mixing method in an internal mixer is provided, wherein the mixing ratio of butyl rubber: 100 parts and liquid polybutene: 16 parts is used.
[0082] The following steps are involved:
[0083] (1) Add all the butyl rubber into an internal mixer and mix for 8 minutes at a pressure of 0.4 MPa.
[0084] (2) adding 8 parts by mass of liquid polybutene and kneading for 10 minutes at a pressure of 0.6 MPa;
[0085] (3) 8 parts by mass of liquid polybutene were added, and the mixture was further kneaded for 10 minutes under a pressure of 0.6 MPa, and then the mixture was discharged.
[0086] (4) Cut the kneaded rubber into strips of 35 cm*6 cm.
[0087] Table 3
[0088]
[0089]
[0090] From Experiment A and Experiment B in Table 3 above, it can be known that the rubber after mixing can improve the efficiency of dissolution, thereby shortening the preparation time of mouse glue.
[0091] Embodiment 4
[0092] Based on the above embodiment, a rubber mixing method in a mixer is provided, wherein the mixing ratio of butyl rubber: 100 parts and liquid polybutene: 24 parts is used for mixing.
[0093] The following steps are involved:
[0094] (1) Add all the butyl rubber into an internal mixer and mix for 8 minutes at a pressure of 0.4 MPa.
[0095] (2) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa;
[0096] (3) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa;
[0097] (4) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa;
[0098] (5) 6 parts by mass of liquid polybutene were added, and the mixture was further kneaded for 8 minutes under a pressure of 0.5 MPa, and then the mixture was discharged.
[0099] (6) Cut the kneaded rubber into strips of 38 cm*7 cm.
[0100] Table 4
[0101]
[0102]
[0103] From Experiment A and Experiment B in Table 4 above, it can be seen that the rubber after mixing can improve the dissolution efficiency, thereby shortening the preparation time of mouse glue.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for mixing rubber in an internal mixer, characterized in that: The following steps are involved: Step 1: Add all the butyl rubber into an internal mixer, and mix them in the internal mixer for 6 to 10 minutes at a pressure of 0.2 to 0.6 MPa; Step 2: Add liquid polybutene to the internal mixer in 2 to 5 equal portions, with an interval of 5 to 10 minutes between each portion, and keep the internal mixer pressure at 0.2 to 0.6 MPa during the internal mixer; Step 3: After the mixing is completed, the material is discharged, cooled, and cut into strips of 30-40cm*4-7cm; Wherein, the mass proportion of the butyl rubber and the liquid polybutene is as follows: Butyl rubber: 100 parts; Liquid polybutene: 15-25 parts.
2. A rubber mixing method in an internal mixer according to claim 1, characterized in that: The mixture was mixed in a mass ratio of 100 parts of butyl rubber and 21 parts of liquid polybutene. The following steps are involved: (1) Add all the butyl rubber into an internal mixer and mix for 6 minutes at a pressure of 0.4 MPa; (2) adding 7 parts by mass of liquid polybutene and kneading for 5 minutes at a pressure of 0.4 MPa; (3) adding 7 parts by mass of liquid polybutene and continuing kneading for 5 minutes at a pressure of 0.4 MPa; (4) adding 7 parts by mass of liquid polybutene, continuing to mix for 5 minutes at a pressure of 0.4 MPa, and discharging; (5) Cut the kneaded rubber into strips of 30 cm*4 cm.
3. A rubber mixing method in an internal mixer according to claim 1, characterized in that: Mix 100 parts of butyl rubber and 25 parts of liquid polybutene in a mixing ratio. The following steps are involved: (1) Add all the butyl rubber into an internal mixer and mix for 10 minutes at a pressure of 0.4 MPa; (2) adding 5 parts by mass of liquid polybutene and kneading for 7 minutes at a pressure of 0.3 MPa; (3) adding 5 parts by mass of liquid polybutene and continuing kneading for 7 minutes at a pressure of 0.3 MPa; (4) adding 5 parts by mass of liquid polybutene and continuing kneading for 7 minutes at a pressure of 0.3 MPa; (5) adding 5 parts by mass of liquid polybutene and continuing kneading for 7 minutes at a pressure of 0.3 MPa; (6) adding 5 parts by mass of liquid polybutene, continuing to mix for 7 minutes at a pressure of 0.3 MPa, and discharging; (7) Cut the kneaded rubber into strips of 35 cm*5 cm.
4. A rubber mixing method in an internal mixer according to claim 1, characterized in that: Mix 100 parts of butyl rubber and 16 parts of liquid polybutene in a mixing ratio. The following steps are involved: (1) Add all the butyl rubber into an internal mixer and mix for 8 minutes at a pressure of 0.4 MPa; (2) adding 8 parts by mass of liquid polybutene and kneading for 10 minutes at a pressure of 0.6 MPa; (3) adding 8 parts by mass of liquid polybutene, continuing to mix for 10 minutes at a pressure of 0.6 MPa, and discharging; (4) Cut the kneaded rubber into strips of 35 cm*6 cm.
5. A rubber mixing method in an internal mixer according to claim 1, characterized in that: Mix 100 parts of butyl rubber and 24 parts of liquid polybutene in a mixing ratio. The following steps are involved: (1) Add all the butyl rubber into an internal mixer and mix for 8 minutes at a pressure of 0.4 MPa; (2) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa; (3) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa; (4) adding 6 parts by mass of liquid polybutene and kneading for 8 minutes at a pressure of 0.5 MPa; (5) adding 6 parts by mass of liquid polybutene, continuing to mix for 8 minutes at a pressure of 0.5 MPa, and discharging; (6) Cut the kneaded rubber into strips of 38 cm*7 cm.
Citation Information
Patent Citations
Small animal trapping material
CN101851474A
Pressure-sensitive adhesive composition for trapping small organisms
CN101959986A
Rat glue having attraction effects, preparation method of the rat glue and rat glue plate coated with the rat glue
CN102850966A
Hot melting mouse-adhibitting adhesive and synthesis method thereof
CN1481677A
Adhesive for capturing small creature
JP2007177105A