A high thermal conductivity and high toughness chlorinated butyl rubber pressure plate
By using materials such as chlorobutyl rubber and boron nitride in the pressure equalizing plate, the problem of insufficient heat resistance and toughness of the existing pressure equalizing plate is solved, and a pressure equalizing plate with high thermal conductivity, high heat resistance and high toughness is realized, which extends the times of use and improves the stability of the product.
Patent Information
- Application Number
- CN202211684202.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The existing pressure equalizing plate has poor heat resistance and insufficient toughness under high temperature and high pressure conditions, resulting in cracking after repeated use. In addition, insufficient thermal conductivity affects the uniform heating of prepregs, resulting in problems such as delamination and bridging of the product.
Chlorinated butyl rubber is used as the main rubber, combined with materials such as boron nitride, to prepare high thermal conductivity and flame retardant chlorinated butyl rubber pressure equalizing plates. By optimizing the formula and process, the thermal conductivity, heat resistance and toughness are improved.
It improves the heat resistance and toughness of the pressure equalizing plate, extends the number of uses, enhances storage stability, and reduces temperature unevenness through thermally conductive fillers, improving the reusability of the product.
Smart Images

Figure CN116003926B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials, and in particular relates to a high-thermal-conductivity and high-toughness chlorinated butyl rubber pressure-equalizing plate. Background Art
[0002] The pressure plate is a very important auxiliary material in the vacuum bag autoclave molding process. It is mainly a plate profile placed on the surface of the prepreg layer. The main function of the pressure plate is to make the prepreg force more uniform, the temperature transfer more stable, and the surface of the cured composite material smoother by relying on the gravity of the pressure plate itself during the prepreg thermal curing process. At present, steel plates, aluminum plates, cardboards, silicone rubber, acrylic rubber, etc. can be used as pressure plates in the tank feeding process.
[0003] During the use of the equalizing plate, the most important thing is to have good ductility, thermal conductivity, heat resistance and a certain degree of flame retardancy. However, in the current aerospace autoclave process auxiliary material market, the equalizing plates provided are often in the high temperature and high pressure vulcanization process of the autoclave. The rubber molecular chains are gradually cross-linked under the action of the vulcanizing agent, but the toughness of the vulcanized equalizing plate (toughness is determined by elongation and strength, the greater the strength, the greater the elongation, the better the toughness) is weak. After repeated use for a period of time, cracks appear at certain arcs and corners, and the characteristic of repeated use is lost. The main reason is that the unvulcanized equalizing plate has poor heat resistance. The equalizing plate made of butyl chloride has better heat resistance. Secondly, the equalizing plate made of butyl bromide has poor storage stability because the bromine element is more active. At the same time, the equalizing plates on the market now have general thermal conductivity during use in the autoclave, and cannot make prepregs such as carbon fiber evenly heated. Therefore, the final product may be differentiated to a certain extent, and delamination, bridging and other symptoms will occur, which will have a certain impact on the final use characteristics of the product.
[0004] At present, patent CN 210560221 U uses butyl bromide as the main rubber in a high thermal conductivity, high wear resistance and flame retardancy composite rubber equalizing plate. The heat resistance is not as good as butyl chloride. The toughness of the vulcanized equalizing plate is weak. After repeated use for a period of time, cracks appear at certain arcs and corners, and the characteristic of multiple reuse is lost. Summary of the invention
[0005] The purpose of the present invention is to provide a high thermal conductivity and high toughness chlorinated butyl rubber equalizing plate in view of the problems existing in the prior art. The present invention uses chlorinated butyl rubber as the main rubber in the formula and combines it with materials such as boron nitride to produce a high thermal conductivity and flame retardant chlorinated butyl rubber equalizing plate.
[0006] The purpose of the present invention can be achieved by the following scheme:
[0007] The present invention provides a high thermal conductivity flame retardant chlorinated butyl rubber pressure equalizing plate, comprising the following components in parts by weight:
[0008]
[0009]
[0010] In one embodiment of the present invention, the reactive rubber comprises one or more of EPDM rubber, butadiene rubber, and styrene butadiene rubber. The reactive rubber is preferably 5-10 parts.
[0011] As an embodiment of the present invention, the butyl rubber includes chlorinated butyl rubber. Butyl rubber has excellent air tightness and waterproofness, and is also resistant to high temperatures and can be used repeatedly.
[0012] As an embodiment of the present invention, the thermally conductive filler includes one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, and silicon carbide. Using a thermally conductive filler helps to dissipate heat at the heating position and reduce the risk of fire or local overheating.
[0013] As an embodiment of the present invention, the flame retardant filler includes one or more of ammonium polyphosphate, melamine, pentaerythritol, and ammonium phosphate salt.
[0014] As one embodiment of the present invention, the tackifying resin includes one or more of C5 petroleum resin, C9 petroleum resin, polyurethane resin, polyester resin, rosin resin, phenolic resin, terpene resin, terpene phenolic resin, coumarone resin, hydrogenated rosin phenol resin, dicyclopentadiene petroleum resin, and styrene resin.
[0015] As an embodiment of the present invention, the plasticizer includes one or more of polyisobutylene, paraffin oil, naphthenic oil, and DINP.
[0016] As an embodiment of the present invention, the vulcanizing agent includes one of sulfur, zinc oxide, and heat-reactive phenolic resin.
[0017] The present invention also provides a method for preparing the high thermal conductivity flame retardant chlorinated butyl rubber pressure equalizing plate, comprising the following steps:
[0018] Step 1: Evenly mix reactive rubber, butyl rubber, thermal conductive filler, flame retardant filler, tackifying resin and plasticizer to prepare a base material;
[0019] Step 2, adding the base material to the vulcanizing agent and kneading to prepare the finished material;
[0020] Step 3: rolling the finished material into sheets, and then rolling it up with the release paper to obtain the high thermal conductivity flame retardant chlorinated butyl rubber equalizing plate.
[0021] As an embodiment of the present invention, in step 1, the mixing temperature is 160-180°C, specifically, the material is stirred and dispersed evenly by an internal mixer, and the internal mixing temperature is less than 180°C.
[0022] As an embodiment of the present invention, in step 2, the kneading temperature is 40-60°C, specifically, a kneading machine with cooling water is used for stirring and dispersing uniformly, and the stirring temperature is less than 60°C.
[0023] As an embodiment of the present invention, in step three, the calendering is performed using a four-roller machine, with the temperature of one roll being 60-70°C, the temperature of the second roll being 50-60°C, the temperature of the third roll being 50-60°C, and the temperature of the first roll being 40-50°C.
[0024] The present invention also provides an application of the high thermal conductivity flame retardant chlorobutyl rubber equalizing plate in a vacuum bag autoclave molding process.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention uses chlorinated butyl rubber as the main material of the rubber layer, which gives the product better heat resistance and toughness, and increases the number of uses and storage stability.
[0027] (2) By using chlorinated butyl rubber and thermal conductive filler (boron nitride has the highest thermal conductivity in the formula, and the use of boron nitride as a thermal conductive filler has the best effect), and further optimizing the content range of each component, an equalizing plate with a thermal conductivity of 2.5 W / MK, a tensile strength of 6.8 MPa, and an elongation at break of 580% was prepared.
[0028] (3) By adopting the inventive method, a pressure equalizing plate with high thermal conductivity, high heat resistance and high toughness can be prepared, which can improve the characteristics of repeated use. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0030] Figure 1 It is a schematic diagram of the structure of the pressure equalizing plate of the present invention when it is rolled up by the release paper;
[0031] Figure 2 It is a schematic diagram of the process of the pressure equalizing plate of the present invention being wound up through the release paper;
[0032] Among them, 1 is the rubber layer and 2 is the release layer. DETAILED DESCRIPTION
[0033] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following examples are implemented on the premise of the technical solution of the present invention, provide detailed implementation methods and specific operation processes, and will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.
[0034] Example 1
[0035] A high thermal conductivity flame retardant chlorobutyl rubber balancing plate. The raw materials of the balancing plate comprise the following components by weight: 9% styrene-butadiene rubber, 24% chlorobutyl rubber, 28.5% boron nitride, 27% ammonium polyphosphate, 6% C5 resin, 5% paraffin oil and 0.5% sulfur.
[0036] The preparation method comprises the following steps:
[0037] Step 1: stir and disperse the reactive rubber, butyl rubber, thermal conductive filler, flame retardant filler, tackifying resin and plasticizer evenly at 170° C. using an internal mixer to prepare a base material;
[0038] Step 2: Add the base material to the vulcanizing agent and knead, use a kneading machine with cooling water to stir and disperse evenly, the stirring temperature is 50°C, and the finished material is prepared;
[0039] Step 3: Roll out the finished product into sheets using a four-roller machine, with one roll at 65°C, two rolls at 55°C, three rolls at 55°C, and one roll at 45°C. Figure 2 As shown in the process, the composite release paper is rolled up, and the structure of the pressure plate after rolling up is as follows Figure 1 As shown, the high thermal conductivity flame retardant chlorinated butyl rubber equalizing plate is obtained, the upper layer is the rubber layer 1, and the lower layer is the release layer 2.
[0040] Example 2
[0041] A high thermal conductivity flame retardant chlorobutyl rubber pressure plate, the raw materials of the pressure plate include the following components by weight percentage: 7% styrene-butadiene rubber, 26% chlorobutyl rubber, 28.5% boron nitride, 27% ammonium polyphosphate, 6% C5 resin, 5% paraffin oil, and 0.5% sulfur. The preparation method is the same as that of Example 1.
[0042] Example 3
[0043] A high thermal conductivity flame retardant chlorobutyl rubber pressure plate, the raw materials of the pressure plate include the following components by weight percentage: 5% styrene-butadiene rubber, 28% chlorobutyl rubber, 28.5% boron nitride, 27% ammonium polyphosphate, 6% C5 resin, 5% paraffin oil, and 0.5% sulfur. The preparation method is the same as that of Example 1.
[0044] Example 4
[0045] A high thermal conductivity flame retardant chlorobutyl rubber pressure plate, the raw materials of the pressure plate include the following components by weight percentage: 3% styrene-butadiene rubber, 30% chlorobutyl rubber, 28.5% boron nitride, 27% ammonium polyphosphate, 6% C5 resin, 5% paraffin oil, and 0.5% sulfur. The preparation method is the same as that of Example 1.
[0046] Example 5
[0047] A high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate. The raw materials of the pressure equalizing plate comprise the following components by weight percentage: 7% EPDM rubber, 26% chlorobutyl rubber, 28.5% magnesium oxide, 27% pentaerythritol, 6% rosin resin, 5% polyisobutylene and 0.5% phenolic resin.
[0048] The preparation method comprises the following steps:
[0049] Step 1: stir and disperse the reactive rubber, butyl rubber, thermal conductive filler, flame retardant filler, tackifying resin and plasticizer evenly at 170° C. using an internal mixer to prepare a base material;
[0050] Step 2: Add the base material to the vulcanizing agent and knead, use a kneading machine with cooling water to stir and disperse evenly, the stirring temperature is 50°C, and the finished material is prepared;
[0051] Step 3: Roll out the finished product into sheets using a four-roller machine, with the temperature of the first roller at 65°C, the temperature of the second roller at 55°C, the temperature of the third roller at 55°C, and the temperature of the first roller at 45°C; roll it up with a composite release paper to obtain the high thermal conductivity flame-retardant chlorobutyl rubber balancing plate. The balancing plate has high thermal conductivity, high heat resistance, and high toughness.
[0052] Comparative Example 1
[0053] A high thermal conductivity flame retardant chlorinated butyl rubber pressure equalizing plate, the raw materials of the pressure equalizing plate are shown in Table 1, brominated butyl rubber is used, and the preparation method is the same as that of Example 1.
[0054] Comparative Example 2
[0055] A high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate, the raw materials of the pressure equalizing plate are shown in Table 1, the styrene butadiene rubber and the chlorobutyl rubber are both 16.5%, and the preparation method is the same as that of Example 1.
[0056] Comparative Example 3
[0057] A high thermal conductivity flame retardant chlorinated butyl rubber pressure equalizing plate, the raw materials of the pressure equalizing plate are shown in Table 1, no styrene-butadiene rubber is added, the chlorinated butyl rubber is 33%, and the preparation method is the same as that of Example 1.
[0058] The following Table 1 compares the specific components of each raw material in the above examples:
[0059] Table 1
[0060]
[0061] The properties of the rubber materials corresponding to the components of Examples 1 to 4 and Comparative Example 1 are shown in Table 2.
[0062] Table 2
[0063]
[0064] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A high thermal conductivity flame retardant chlorinated butyl rubber pressure plate, characterized in that: The composition comprises the following components in parts by weight: 3-10 parts of reactive rubber; Butyl rubber 25-35 parts; 25-35 parts of thermal conductive filler; 25-35 parts of flame retardant filler; 5-10 parts of tackifying resin; 3-10 parts of plasticizer; Vulcanizing agent 0.3-3 parts; The reactive rubber is one or more of EPDM rubber, butadiene rubber, and styrene-butadiene rubber; The butyl rubber is chlorinated butyl rubber.
2. The high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate according to claim 1, characterized in that: The thermal conductive filler includes one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, and silicon carbide.
3. The high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate according to claim 1, characterized in that: The flame retardant filler includes one or more of ammonium phosphate salt and ammonium polyphosphate.
4. The high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate according to claim 1, characterized in that: The tackifying resin includes one or more of C5 petroleum resin, C9 petroleum resin, polyurethane resin, polyester resin, rosin resin, phenolic resin, terpene resin, coumarone resin, hydrogenated rosin phenol resin, and styrene resin.
5. The high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate according to claim 1, characterized in that: The plasticizer includes one or more of polyisobutylene, paraffin oil, naphthenic oil, and DINP.
6. The high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate according to claim 1, characterized in that: The vulcanizing agent includes one of sulfur, metal oxide and phenolic resin.
7. A method for preparing the high thermal conductivity flame retardant chlorobutyl rubber pressure equalizing plate according to claim 1, comprising the following steps: Step 1: Evenly mix reactive rubber, butyl rubber, thermal conductive filler, flame retardant filler, tackifying resin and plasticizer to prepare a base material; Step 2, adding the base material to the vulcanizing agent and kneading to prepare the finished material; Step 3: rolling the finished material into sheets, and then rolling it up with the release paper to obtain the high thermal conductivity flame retardant chlorinated butyl rubber equalizing plate.
8. Use of the high thermal conductivity flame retardant chlorobutyl rubber equalizing plate as claimed in claim 1 in a vacuum bag autoclave molding process.
Citation Information
Patent Citations
High-thermal-conductivity, high-wear-resistance and flame-retardant composite rubber pressure equalizing plate
CN210560221U
In-situ polymerization reinforced high-thermal-conductivity rubber-based composite and preparation method thereof
CN105315564A
Heat-conducting sound-proof rubber sheet and preparation method thereof
CN107973943A
Vulcanized butyl pressure-sensitive adhesive
CN110184003A
Low-aldehyde automobile butyl damping fin and preparation method thereof
CN111378233A