Polishing liquid and preparation method thereof, and polishing method for metal parts

By using a combination of phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor and active diol in the polishing liquid, the problem of uneven polishing of traditional polishing liquid is solved, significantly improving the polishing effect of aluminum alloy products and reducing the The phenomenon of surface flowers and flow marks improves the surface quality.

CN116005159BActive Publication Date: 2024-11-22CHANGSHA YONGAN NEW MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211604594.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-22
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Traditional polishing liquids are prone to unevenness when polishing the surface of aluminum alloy products, resulting in appearance problems such as surface flowers and flow marks, affecting the surface quality of the product.

Method used

Using a polishing liquid including a polishing base liquid and a gas mark inhibitor, which consists of phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor and active diol, mixed by optimizing component ratio and temperature conditions , a polishing liquid is formed to improve polishing uniformity and stability.

Benefits of technology

It effectively improves the polishing effect of the polishing liquid, reduces the surface flower and flow marks, improves the surface gloss and brightness uniformity of the metal parts, and enhances the stability and cleaning ability of the polishing liquid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present disclosure relates to a polishing liquid and a preparation method thereof, and a polishing method for metal parts. The polishing liquid includes a polishing base liquid and a gas mark inhibitor, and the gas mark inhibitor includes phosphoric acid, m-nitrobenzene sulfonate, a corrosion inhibitor, an active diol and water. The technical solution disclosed in the present disclosure effectively solves the technical problem that the conventional polishing liquid polishes unevenly, resulting in poor appearance problems such as surface spots and flow marks on the metal surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal surface treatment, and in particular to a polishing liquid and a preparation method thereof, and a polishing method for metal parts. Background Art

[0002] With the development of science and technology, the replacement speed of electronic products is getting faster and faster, and the material of the electronic product frame has gradually changed from plastic to metal. Among them, aluminum alloy is widely used in the electronic product industry due to its unique advantages such as light weight, low price and good metal performance.

[0003] In the related art, when preparing aluminum alloy products, in order to improve their decorative properties, it is usually necessary to perform surface treatments such as polishing on the aluminum alloy products so that the aluminum alloy products have a more beautiful appearance and durability. However, when polishing the surface of the aluminum alloy products, the chemical solution polishing is uneven, resulting in appearance problems such as surface spots and flow marks on the surface of the aluminum alloy products, which seriously affects the surface quality of the aluminum alloy products. Summary of the invention

[0004] The present invention provides a polishing liquid and a preparation method thereof, and a polishing method for metal parts, so as to solve the technical problem that the conventional polishing liquid polishes unevenly, resulting in surface spots and flow marks on the metal surface and other undesirable appearance effects.

[0005] To this end, in a first aspect, the present disclosure provides a polishing liquid, including a polishing base liquid and a gas mark inhibitor, wherein the gas mark inhibitor includes phosphoric acid, m-nitrobenzene sulfonate, a corrosion inhibitor, an active diol and water.

[0006] In a possible implementation, the mass percentages of the components in the gas mark inhibitor are:

[0007] Phosphoric acid 75%~85%;

[0008] m-nitrobenzene sulfonate 0.1%~1%;

[0009] Corrosion inhibitor 1%~5%;

[0010] Active diol 0.1%~0.5%;

[0011] The rest is water;

[0012] Among them, the mass ratio between m-nitrobenzene sulfonate and active diol is (1.8~2.2):1.

[0013] In a possible implementation, the corrosion inhibitor is one or more of thiourea, propyl sulfide, diamylamine or formaldehyde.

[0014] In a possible implementation manner, the mass ratio between m-nitrobenzene sulfonate and active diol is (1.8-2.2):1.

[0015] In a specific embodiment, the mass ratio between the m-nitrobenzene sulfonate and the active diol is 2:1.

[0016] In a possible implementation, the polishing base liquid includes sulfuric acid and phosphoric acid, wherein the volume ratio of sulfuric acid to phosphoric acid is 2:(5-7).

[0017] In a possible implementation, the active diol is one or more of polyethylene glycol and sorbitol.

[0018] In a second aspect, the present disclosure further provides a method for preparing a polishing liquid, comprising:

[0019] Mix sulfuric acid and phosphoric acid to obtain a polishing base solution;

[0020] Phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor, active diol and water are mixed to obtain a gas mark inhibitor;

[0021] At a temperature of 70° C. to 80° C., the gas mark inhibitor is added into the polishing base liquid and mixed to obtain a target polishing liquid.

[0022] In a possible implementation, the step of mixing phosphoric acid, m-nitrobenzene sulfonate, a corrosion inhibitor, an active diol and water to obtain a gas mark inhibitor comprises:

[0023] Adding m-nitrobenzene sulfonate into water to dissolve it, then adding active diol and mixing well to obtain a first solution;

[0024] Add the corrosion inhibitor into part of the phosphoric acid to dissolve and mix well to obtain a second solution;

[0025] The first solution, the second solution and the remaining phosphoric acid are mixed to obtain a gas mark inhibitor.

[0026] In a possible implementation, the mass percentages of the components in the gas mark inhibitor are: phosphoric acid 75% to 85%; m-nitrobenzene sulfonate 0.1% to 1%; corrosion inhibitor 1% to 5%; active diol 0.1% to 0.5%; and the rest is water.

[0027] In a third aspect, the present disclosure further provides a method for polishing a metal part, comprising:

[0028] After immersing the metal part in the polishing liquid as described above for 50s to 70s, the metal part is taken out, cleaned, and dried to obtain a polished metal part; wherein the temperature of the polishing liquid is 60°C to 80°C.

[0029] According to the polishing liquid and its preparation method, and the polishing method of metal parts provided by the present disclosure, the polishing liquid includes a polishing base liquid and a gas mark inhibitor, and the gas mark inhibitor includes phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor, active diol and water. The technical scheme disclosed in the present disclosure optimizes the specific components of the polishing liquid to improve the polishing uniformity of the metal part surface by the polishing liquid, and reduce the appearance problems such as surface spots and flow marks on the metal surface. Specifically, the gas mark inhibitor adopts phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor and active diol to solve the problem of uneven polishing of metal parts by traditional polishing liquid, and effectively improves the polishing effect of the polishing liquid. At the same time, the combination of m-nitrobenzene sulfonate and active diol is conducive to removing the oxide layer and dirty substances on the surface of the metal part, so that the contact between the polishing liquid and the surface of the metal part is more uniform and the reaction is more uniform; and, through the combination of active diol and corrosion inhibitor, the reaction between the polishing liquid and the surface of the metal part is warmer and the polishing stability is stronger. In this way, the polishing performance and polishing effect of the polishing liquid are effectively improved, and the appearance problems such as surface spots and flow marks that are prone to appear on the surface of metal parts after polishing are effectively improved. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution in the embodiments of the present disclosure will be clearly and completely described below in combination with the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present disclosure.

[0031] The embodiment of the present disclosure provides a polishing liquid, including a polishing base liquid and a gas mark inhibitor, wherein the gas mark inhibitor includes phosphoric acid, m-nitrobenzene sulfonate, a corrosion inhibitor, an active diol and water.

[0032] In this embodiment, the specific components of the polishing liquid are optimized to improve the polishing uniformity of the metal surface by the polishing liquid, thereby reducing the appearance problems such as surface spots and flow marks on the metal surface.

[0033] Specifically, the gas mark inhibitor is configured as a composite component including at least phosphoric acid, m-nitrobenzene sulfonate, a corrosion inhibitor and an active diol. The synergistic cooperation between the composite components effectively solves the problem of uneven polishing of metal parts by traditional polishing liquids, and improves the polishing effect of the polishing liquid.

[0034] The m-nitrobenzene sulfonate can remove the oxide layer on the metal surface and reduce the deposition of the metal oxide layer on the metal surface, so as to improve the contact uniformity between the gas mark inhibitor and the metal surface. Specifically, the nitro group in the m-nitrobenzene sulfonate can undergo a reduction reaction with the metal oxide layer, thereby achieving the effect of removing the oxide film layer on the surface of the metal polishing part, increasing the effective contact area between the gas mark inhibitor and the metal polishing part, and thus improving the polishing effect. At the same time, the m-nitrobenzene sulfonate has acid resistance and is easily soluble in water, so that the m-nitrobenzene sulfonate is evenly distributed in the polishing liquid, which is conducive to improving the uniformity of the polishing liquid on the surface oxide layer of the metal polishing part, avoiding the phenomenon that a part of the surface of the metal polishing part has been polished / polished transition, and another part is still not polished, thereby improving the polishing effect of the metal part.

[0035] The active diol can increase the wettability of the polishing liquid on the metal surface, thereby increasing the reaction area between the polishing liquid and the metal surface, increasing the polishing reaction speed, and improving the polishing effect; at the same time, the active diol is also beneficial to reduce the activation energy of the interface reaction between the polishing liquid and the metal, reduce the surface tension of the polishing liquid, and improve the cleaning ability and stability of the polishing liquid; and the active diol can also improve the antistatic effect of the polishing liquid. At the same time, through the coordination of m-nitrobenzene sulfonate and active diol, the dispersing and wetting effects of the active diol are utilized to make the contact between m-nitrobenzene sulfonate and the surface of the metal part more complete, so that it is beneficial to remove the oxide layer and dirty substances on the surface of the metal part, and make the contact between the polishing liquid and the surface of the metal part more uniform and the reaction more uniform. The corrosion inhibitor can improve the gas mark problem caused by uneven polishing intensity during the polishing process, slow down the corrosion efficiency of phosphoric acid on the surface of the metal part, and buffer the corrosion effect of the polishing liquid on the surface of the metal part. At the same time, by combining the active diol with the corrosion inhibitor, the dispersing and wetting properties of the active diol are utilized to make the corrosion inhibitor more evenly dispersed, so that the corrosion inhibitor and the metal parts are in more complete and comprehensive contact. In addition, the corrosion inhibitor can reduce the corrosion efficiency of the polishing liquid on the surface of the metal parts. Therefore, the corrosion inhibitor evenly dispersed in the polishing liquid can make the reaction between the polishing liquid and the surface of the metal parts warmer and the polishing stability stronger. In this way, the polishing performance and polishing effect of the polishing liquid are effectively improved, and the appearance problems such as surface spots and flow marks that are easy to appear on the surface of the metal parts after polishing are effectively improved.

[0036] In a specific example, the active diol is polyethylene glycol. The addition of active diol in the gas mark inhibitor can improve the compatibility of the components in the polishing liquid and make the dispersion of the substances in the polishing liquid more uniform. Of course, in other embodiments, the active diol can also be other surfactants, such as sorbitol.

[0037] In a possible implementation, the mass percentages of the components in the gas mark inhibitor are:

[0038] Phosphoric acid 75%~85%;

[0039] m-nitrobenzene sulfonate 0.1%~1%;

[0040] Corrosion inhibitor 1%~5%;

[0041] Active diol 0.1%~0.5%;

[0042] The rest is water;

[0043] Among them, the mass ratio between m-nitrobenzene sulfonate and active diol is (1.8~2.2):1.

[0044] In this embodiment, the addition range of each component in the gas mark inhibitor is set so that the components in the gas mark inhibitor can exert the maximum synergistic effect. Among them, the phosphoric acid is phosphoric acid with a mass concentration of 85%.

[0045] In a specific example,

[0046] In a possible embodiment, the corrosion inhibitor is one or more of thiourea, propyl sulfide, diamylamine or formaldehyde. For example, but not limited to, the corrosion inhibitor is thiourea.

[0047] In a possible embodiment, the m-nitrobenzene sulfonate is one or more of sodium m-nitrobenzene sulfonate, potassium m-nitrobenzene sulfonate, calcium m-nitrobenzene sulfonate, and magnesium m-nitrobenzene sulfonate.

[0048] In a possible embodiment, the mass ratio of m-nitrobenzene sulfonate to active diol is (1.8-2.2): 1. For example but not limited to, the mass ratio of m-nitrobenzene sulfonate to active diol is 2:1.

[0049] In a possible implementation, the polishing base liquid includes sulfuric acid and phosphoric acid, wherein the volume ratio of sulfuric acid to phosphoric acid is 2:(5-7). For example but not limited to, the volume ratio of sulfuric acid to phosphoric acid is 2:6.

[0050] In a possible embodiment, the active diol is one or more of polyethylene glycol and sorbitol. For example, but not limited to, the active diol is polyethylene glycol.

[0051] In a possible implementation manner, the volume proportion of the gas mark inhibitor in the polishing liquid is 2% to 3%.

[0052] In a second aspect, the present disclosure further provides a method for preparing a polishing liquid, comprising:

[0053] Mix sulfuric acid and phosphoric acid to obtain a polishing base solution;

[0054] Phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor, active diol and water are mixed to obtain a gas mark inhibitor;

[0055] At a temperature of 70° C. to 80° C., the gas mark inhibitor is added into the polishing base liquid and mixed to obtain a target polishing liquid.

[0056] In this embodiment, the polishing base liquid and the gas mark inhibitor need to be separately prepared first, and then the prepared polishing base liquid and the gas mark inhibitor are mixed at a certain temperature to obtain the target polishing liquid.

[0057] In the preparation of the polishing base liquid, sulfuric acid and phosphoric acid in a certain ratio (such as a volume ratio of 2:6) need to be weighed separately, and then sulfuric acid is slowly added to phosphoric acid and mixed to obtain the polishing base liquid. Among them, sulfuric acid is sulfuric acid with a mass concentration of 90%, and phosphoric acid is phosphoric acid with a mass concentration of 85%.

[0058] In a possible implementation, the step of mixing phosphoric acid, m-nitrobenzene sulfonate, a corrosion inhibitor, an active diol and water to obtain a gas mark inhibitor comprises:

[0059] Adding m-nitrobenzene sulfonate into water to dissolve it, then adding active diol and mixing well to obtain a first solution;

[0060] Add the corrosion inhibitor into part of the phosphoric acid to dissolve and mix well to obtain a second solution;

[0061] The first solution, the second solution and the remaining phosphoric acid are mixed to obtain a gas mark inhibitor.

[0062] In this embodiment, the preparation method of the gas mark inhibitor is further optimized. Specifically, m-nitrobenzene sulfonate is first added to water to dissolve, and then an active diol is added, reacted, and mixed to obtain a first solution. Then, the corrosion inhibitor is added to 1 / 2 of phosphoric acid, reacted, dissolved, and mixed to obtain a second solution. Finally, the first solution, the second solution, and the remaining 1 / 2 of phosphoric acid are mixed to obtain a gas mark inhibitor.

[0063] In a possible implementation, the mass percentages of the components in the gas mark inhibitor are: phosphoric acid 75% to 85%; m-nitrobenzene sulfonate 0.1% to 1%; corrosion inhibitor 1% to 5%; active diol 0.1% to 0.5%; and the rest is water.

[0064] In a third aspect, the present disclosure further provides a method for polishing a metal part, comprising:

[0065] After immersing the metal part in the polishing liquid as described above for 50s to 70s, the metal part is taken out, cleaned, and dried to obtain a polished metal part; wherein the temperature of the polishing liquid is 60°C to 80°C.

[0066] To further illustrate the beneficial effects of the polishing liquid provided by the present disclosure, the following is an explanation in conjunction with a specific embodiment group. It should be understood that the specific embodiment group is a further detailed description of the present disclosure and does not limit the protection scope of the present disclosure. At the same time, the raw materials and equipment used in the embodiment group can be purchased on the market.

[0067] Example Group 1

[0068] 1. Preparation of polishing liquid:

[0069] ① Weigh sulfuric acid and phosphoric acid in a volume ratio of 2:6 respectively, and then mix them to obtain a polishing base liquid.

[0070] ② Weigh phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor, active diol and water respectively according to the mass ratio in Table 1; then, add m-nitrobenzene sulfonate into water to dissolve, then add active diol and mix well to obtain a first solution; then, add corrosion inhibitor into 1 / 2 of phosphoric acid and mix well to obtain a second solution; finally, mix the first solution, the second solution and the remaining 1 / 2 of phosphoric acid to obtain a gas mark inhibitor.

[0071] ③ Under the temperature condition of 70°C to 80°C, add the gas mark inhibitor into the polishing base liquid and mix well to obtain the target polishing liquid, wherein the volume proportion of the gas mark inhibitor in the polishing liquid is 2.5%.

[0072] Table 1 Gas trace inhibitor groups with different contents

[0073]

[0074] 2. Performance test of polishing fluid:

[0075] Multiple metal parts (aluminum alloy frames) of the same size and surface area were placed in the polishing liquid prepared according to the gas mark inhibitor in Table 1, polished at 75°C for 1 min, and taken out; the aluminum alloy frame was then cleaned and dried with pure water, and the gas mark and surface condition of the polished aluminum alloy frame was tested. The test results are shown in Table 2.

[0076] Table 2 Polishing effect of aluminum alloy frame under different polishing liquids

[0077]

[0078] 3. Result analysis:

[0079] According to Tables 1 and 2, when the mass ratio of m-nitrobenzene sulfonate to active diol in the polishing liquid is not (1.8~2.2):1, such as control group 1, 5% of the metal parts have uneven brightness, and 5% of the metal parts have gas marks on the surface; when the polishing liquid does not contain active diol, and the content of phosphoric acid and thiourea is too high, such as control group 2, 15% of the metal parts have uneven brightness, and 10% of the metal parts have gas marks on the surface; when the metal parts are polished with pure phosphoric acid, such as control group 3, 10% of the metal parts have uneven brightness, and 25% of the metal parts have gas marks on the surface; when the content of thiourea in the polishing liquid is too high, such as control group 4, 5% of the metal parts have uneven brightness, and 10% of the metal parts have gas marks on the surface; when m-nitrobenzene sulfonate does not exist in the polishing liquid, and the content of phosphoric acid, thiourea and active diol in the polishing liquid is too high, such as control group 5, 20% of the metal parts have uneven brightness, and 10% of the metal parts have gas marks on the surface.

[0080] The aluminum alloy frame polished by the polishing liquid provided in the present disclosure has a glossiness higher than 100, no air marks on the surface, uniform brightness, and no surface fringing. Therefore, the polishing liquid provided in the present disclosure can effectively improve the air marks and surface fringing on the surface of metal parts and improve the polishing effect of metal parts.

[0081] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0082] The above description is only a specific embodiment of the present disclosure, so that those skilled in the art can understand or implement the present disclosure. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A polishing liquid, It is characterized in that It comprises a polishing base liquid and a gas mark inhibitor, wherein the gas mark inhibitor comprises phosphoric acid, m-nitrobenzene sulfonate, a corrosion inhibitor, an active diol and water; wherein the mass percentage of each component in the gas mark inhibitor is: Phosphoric acid 75%~85%; m-nitrobenzene sulfonate 0.1%~1%; Corrosion inhibitor 1%~5%; Active diol 0.1%~0.5%; The rest is water; The mass ratio of the m-nitrobenzene sulfonate to the active diol is (1.8-2.2):1, and the active diol is one or more of polyethylene glycol or sorbitol.

2. The polishing liquid according to claim 1, It is characterized in that The corrosion inhibitor is one or more of thiourea, propyl sulfide, diamylamine or formaldehyde.

3. The polishing liquid according to claim 1, It is characterized in that The mass ratio between the m-nitrobenzene sulfonate and the active diol is 2:

1.

4. The polishing liquid according to claim 1, It is characterized in that The polishing base liquid includes sulfuric acid and phosphoric acid, wherein the volume ratio of the sulfuric acid to the phosphoric acid is 2:(5-7).

5. A method for preparing the polishing liquid according to any one of claims 1 to 4, It is characterized in that include: Mix sulfuric acid and phosphoric acid to obtain a polishing base solution; Phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor, active diol and water are mixed to obtain a gas mark inhibitor; Under the temperature condition of 70° C. to 80° C., the gas mark inhibitor is added into the polishing base liquid and mixed to obtain the target polishing liquid.

6. The preparation method according to claim 5, It is characterized in that The step of mixing phosphoric acid, m-nitrobenzene sulfonate, corrosion inhibitor, active diol and water to obtain a gas mark inhibitor comprises: Adding m-nitrobenzene sulfonate into water to dissolve it, then adding active diol and mixing well to obtain a first solution; Add the corrosion inhibitor into part of the phosphoric acid to dissolve, mix well, and obtain a second solution; The first solution, the second solution and the remaining phosphoric acid are mixed to obtain the gas mark inhibitor.

7. A method for polishing a metal part, It is characterized in that include: After immersing the metal part in the polishing liquid as described in any one of claims 1 to 4 for 50 seconds to 70 seconds, taking it out, cleaning it, and drying it to obtain a polished metal part; wherein the temperature of the polishing liquid is 60°C to 80°C.

Citation Information

Patent Citations

  • Polishing solution

    CN105734574A

  • Alkalescent copper polishing solution

    CN105885701A

  • Smokeless polishing solution for aluminum products

    CN107177848A

  • Environmental-protection energy-saving chemical polishing liquid and polishing method thereof

    CN107653452A