A method and application of a catalyst for constructing a local alkaline environment
By introducing a hard Lewis acid layer on the catalyst surface, a local alkaline environment is constructed, which solves the problem of poor catalytic performance under neutral pH conditions, significantly improves the performance of various electrocatalytic reactions, reduces production costs, and achieves wide application.
Patent Information
- Application Number
- CN202310023265.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-01-09
AI Technical Summary
Under neutral pH conditions, the catalytic performance of electrocatalytic reactions is poor, the reaction rate is slow, and the current is low. The existing methods of constructing a local alkaline environment are limited and difficult to adapt to a variety of catalysts and reactions.
By introducing a hard Lewis acid layer on the catalyst surface and using Cr2O3 and TiO2 as Lewis acids, the transition metal oxide catalyst is modified to create a local alkaline environment, which is suitable for a variety of catalysts and reactions.
It significantly improves the performance of hydrogen evolution, oxygen evolution and carbon dioxide reduction reactions in neutral electrolytes, reduces production costs, and achieves long-term stability and widespread application of the catalyst.
Smart Images

Figure CN116005190B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrocatalysis, and in particular relates to a method and application of a catalyst for constructing a local alkaline environment. Background Art
[0002] Compared with the commonly used alkaline electrolytes, neutral electrolytes have milder reaction conditions and more convenient application scenarios, which is conducive to the electrocatalytic system to maintain good catalytic stability after long-term reaction, while reducing production costs (>800US$t -1 KOH), to achieve a wider range of household applications. However, the catalytic performance of most electrochemical reactions (such as hydrogen evolution and oxygen evolution reactions) at neutral pH is far inferior to that at alkaline pH, with slow reaction rates and low currents. This is mainly attributed to the poor water dissociation ability and too low hydrogen / hydroxyl concentrations under neutral pH conditions. Recent work in the field of electrocatalysis has shown that by constructing a local alkaline environment in a neutral electrolyte (usually on the catalyst surface), it is expected to solve the problems of slow kinetics and low current under neutral pH conditions. This has been proven in the field of electrocatalytic carbon dioxide reduction: the local hydroxide ion concentration will significantly improve the adsorption configuration of reaction intermediates and the selectivity of products, and plays a vital role in determining the reaction mechanism and improving the reaction performance. However, the current methods for constructing a local alkaline environment are still very limited, mainly using physical methods, such as the electrode preparation engineering in the carbon dioxide electroreduction reaction reported in the literature: usually by optimizing the physical properties of the electrode such as pore size, thickness, roughness, hydrophilicity / hydrophobicity, etc., to adjust the dissociation / generation process of bicarbonate in the electrolyte [References 1, 2, 3], thereby regulating the pH near the click. However, this method is only applicable to reactions such as carbon dioxide electroreduction with carbonate / bicarbonate as electrolyte, and has strict requirements on the morphology of the electrode (limited to electrodes with a wide range of pore size and roughness). Therefore, it is crucial to develop a more general method for constructing a local alkaline environment to accommodate a wider range of catalysts and reactions.
[0003] According to the Lewis acid-base theory, Lewis acid has the advantage of quickly dissociating water molecules and capturing hydroxide ions. Therefore, we believe that through Lewis acid modification, it is possible to construct a local alkaline environment on the surface of commonly used electrocatalysts, thereby realizing their application in different catalysts and different catalytic reactions.
[0004] References
[0005] 1. High-aspect-ratio Ag nanowire mat electrodes for electrochemical COproduction from CO2. ACS Catalysis, 2021, 11(19): 11945-11959.
[0006] 2.Competition between CO2 reduction and hydrogen evolution on a goldelectrode under well-defined mass transport conditions. Journal of the American Chemical Society, 2020, 142(9): 4154-4161.
[0007] 3.Address the “alkalinity problem” in CO2 electrolysis with catalystdesign and translation[J].Joule,2021,5(4):737-742. Summary of the invention
[0008] In order to solve the problems of the prior art, the present invention provides the following technical solutions:
[0009] The present invention provides a method for constructing a catalyst with a local alkaline environment. A series of substrate catalysts construct a local alkaline environment on the surface of the substrate catalyst by introducing a hard Lewis acid layer, without relying on an alkaline electrolyte.
[0010] In the present invention, the substrate catalyst has a wide range of applicability. Most catalysts with high reaction activity, such as transition metal oxides such as CoO x , NiO x and MnO x etc., x represents the different valence states of transition metal ions; and precious metals such as Pt and RuO2 can be used as substrate catalysts.
[0011] In the present invention, both Cr2O3 and TiO2 can act as Lewis acids to rapidly dissociate water molecules on the surface of the substrate catalyst and capture hydroxide ions. The only difference is the strength of the Lewis acid. In the transition metal oxide catalyst modified by the Lewis acid, the atomic percentage of Cr is 2-20%; the atomic percentage of Ti is 5-35%.
[0012] In the present invention, the preparation of the Lewis acid-modified substrate catalyst comprises the following steps: preparing a Cr2O3 / TiO2 precursor solution, impregnating, and vacuum annealing. Specifically:
[0013] (1) The Cr2O3 precursor solution is an ethanol solution of chromium nitrate with a concentration of 0.02-0.5M; the TiO2 precursor solution is a titanium isopropoxide solution with a concentration of 0.05-0.6M;
[0014] (2) The substrate catalyst transition metal oxide (such as transition metal oxide: CoO x , NiO x and MnO x etc. Precious metals: Pt and RuO2 etc. are immersed in the precursor solution for 0.5-1.5min and then taken out and dried;
[0015] (3) The vacuum annealing process is carried out in a vacuum tube furnace under argon / nitrogen protection; the annealing temperature is set at 375-425°C, the rate of heating from room temperature to the set temperature is 5-10°C / min, and the temperature is kept for 2.5-3.5 hours; the vacuum degree is less than 3.0×10 -1 Entrust.
[0016] The catalyst prepared by the method for constructing a catalyst in a local alkaline environment of the present invention is applied to the electrocatalytic reaction of hydrogen evolution, oxygen evolution or carbon dioxide reduction.
[0017] In the present invention, the hydrogen and oxygen evolution performance of the substrate catalyst modified by Cr2O3 or TiO2 was tested in a neutral electrolyte: a three-electrode electrochemical system test was performed using a CHI 660E electrochemical workstation. x , NiO x and MnO x etc.) as the working electrode, the carbon rod as the counter electrode, and the calomel electrode (SCE) as the reference electrode. SCE Convert to E RHE The calculation formula is: E RHE =E SCE +0.71V.
[0018] (1) Hydrogen evolution performance test: The electrolyte is natural seawater saturated with nitrogen (neutral, pH = 7.9), and the nitrogen atmosphere is maintained during the reaction. First, the cyclic voltammetry (CV) curve is tested until it coincides: voltage range: -0.61 ~ (-1.01)
[0019] VSCE, scan rate: 50 mV s -1 ; Then test the polarization curve linear sweep voltammetry (LSV) curve: voltage range: -0.61 ~ (-1.01) V SCE, scan rate: 5mV s -1 ;
[0020] (2) Oxygen evolution performance test: The electrolyte is natural seawater saturated with oxygen (neutral, pH = 7.9), and the oxygen atmosphere is maintained during the reaction. First, the cyclic voltammetry (CV) curve is tested until it coincides: voltage range: 0.49-1.29VSCE, scan rate: 50mV s -1; Then test the polarization curve linear sweep voltammetry (LSV) curve: voltage range: 0.49~1.29VSCE, scan rate: 5mV s -1 ;
[0021] In the present invention, the substrate catalyst (such as transition metal oxide: CoO x , NiO x and MnO x After modification with Cr2O3 or TiO2, the performance of hydrogen and oxygen evolution in neutral electrolytes has been greatly improved. x It exhibits the best hydrogen and oxygen evolution performance: at a current density of 10 mA cm-2, it is comparable to pure CoO x Compared with the catalyst, Cr2O3-CoO x The overpotentials of hydrogen evolution and oxygen evolution of the catalyst decreased by 0.22 and 0.31 V respectively. The actual overpotential of hydrogen evolution was only 0.10 V; the overpotential of oxygen evolution was only 0.46 V.
[0022] The method of the present invention can construct a local alkaline reaction environment under neutral pH conditions without the need to add alkali (KOH). This is beneficial for the electrocatalytic system to maintain good catalytic stability after long-term reaction, while reducing production costs (>800 US$t -1 KOH), to achieve a wider range of household applications. This modification method is applicable to various commonly used substrate catalysts in catalytic reactions (such as transition metal oxides: CoO x , NiO x and MnO x The Cr2O3-modified catalyst can significantly improve the catalytic performance of the above reactions in neutral electrolytes (pure water, natural seawater, weakly buffered salt solutions), and even approach the reaction performance in alkaline electrolytes. x It exhibits the best hydrogen and oxygen evolution performance: at a current density of 10 mA cm-2, it is comparable to pure CoO x Compared with the catalyst, Cr2O3-CoO x The overpotentials of hydrogen evolution and oxygen evolution of the catalyst decreased by 0.22 and 0.31 V respectively. The actual overpotential of hydrogen evolution was only 0.10 V; the overpotential of oxygen evolution was only 0.46 V. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 : Cr2O3 modified CoO x Morphology of the catalyst: a, scanning image; b, transmission image;
[0024] Figure 2 :TiO2 modified CoO x Morphology of the catalyst: a, scanning image; b, transmission image;
[0025] Figure 3 :In natural seawater (pH~8), CoO x and Cr2O3 modified CoO x The local pH changes of the cathode (hydrogen evolution reaction) and anode (oxygen evolution reaction) during the electrolysis of water: a represents the local pH change of the anode surface during the oxygen evolution process, and b represents the pH change of the cathode surface during the hydrogen evolution process;
[0026] Figure 4 :CoO x and Cr2O3 modified CoO x Comparison of hydrogen and oxygen evolution performance of catalysts in natural seawater (pH ~ 8): a represents the oxygen evolution performance curve, and b represents the hydrogen evolution performance curve;
[0027] Figure 5 : Cr2O3 modified NiO x , MnO x and TiO2-modified CoO x Oxygen evolution performance of the catalyst in natural seawater (pH ~ 8): In the figure, a represents Cr2O3-NiO x Oxygen evolution performance curve, b represents Cr2O3-MnO x Oxygen evolution performance curve, c represents TiO2-CoO x Oxygen evolution performance curve. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0029] Example 1: Cr2O3-modified CoO x Catalyst preparation
[0030] (1) Preparation of Cr2O3 precursor solution: dissolve 0.1 M chromium nitrate in ethanol and stir by ultrasonic until the mixture is uniform;
[0031] (2) The substrate catalyst CoO loaded on carbon paper / conductive glass x Immersed in Cr2O3 precursor solution for 1
[0032] min and then dried at room temperature.
[0033] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 400°C at a heating rate of 10°C / min, then kept at this temperature for 3 h, and then cooled to room temperature with the furnace; thus, Cr2O3-modified CoO x Catalyst. Cr2O3-CoO x The morphology of the catalysts was characterized by Figure 1 .in, Figure 1 a means scanned image, Figure 1 b indicates transmission image
[0034] Cr2O3 modified CoO x The atomic percentage of Cr in the catalyst is 6%.
[0035] Example 2: Cr2O3 modified NiO x Catalyst preparation
[0036] (1) Preparation of Cr2O3 precursor solution: dissolve 0.02M chromium nitrate in ethanol and stir by ultrasonic until the mixture is uniform;
[0037] (2) The substrate catalyst NiO supported on carbon paper / conductive glass x Immersed in Cr2O3 precursor solution for 0.5
[0038] min and then dried at room temperature.
[0039] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 400°C at a heating rate of 10°C / min, then kept at this temperature for 3 h, and then cooled to room temperature in the furnace; thus, Cr2O3-modified NiO was obtained. x catalyst.
[0040] Cr2O3 modified NiO x The atomic percentage of Cr in the catalyst is 2%.
[0041] Example 3: Cr2O3 modified MnO x Catalyst preparation
[0042] (1) Preparation of Cr2O3 precursor solution: dissolve 0.02M chromium nitrate in ethanol and stir by ultrasonic until the mixture is uniform;
[0043] (2) The substrate catalyst MnO supported on carbon paper / conductive glass x Immerse in Cr2O3 precursor solution for 0.5 min and then dry at room temperature.
[0044] (3) Annealing: The sample was placed in a vacuum tube furnace and annealed under nitrogen protection: heated to 400°C at a heating rate of 10°C / min, then kept at this temperature for 3 h, and then cooled to room temperature with the furnace; thus, Cr2O3-modified MnO x catalyst.
[0045] Cr2O3 modified MnO x The atomic percentage of Cr in the catalyst is 2%.
[0046] Example 4: Preparation of Cr2O3-modified Pt catalyst
[0047] (1) Preparation of Cr2O3 precursor solution: dissolve 0.5 M chromium nitrate in ethanol and stir by ultrasonic until the mixture is uniform;
[0048] (2) The substrate catalyst Pt supported on carbon paper / conductive glass was immersed in the Cr2O3 precursor solution for 1.5
[0049] min and then dried at room temperature.
[0050] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 375°C at a heating rate of 5°C / min, then kept warm for 2.5 h, and then cooled to room temperature in the furnace; thus, a Cr2O3-modified Pt catalyst was obtained.
[0051] In the Cr2O3-modified Pt catalyst, the atomic percentage of Cr is 20%.
[0052] Example 5: Preparation of Cr2O3-modified RuO2 catalyst
[0053] (1) Preparation of Cr2O3 precursor solution: dissolve 0.2 M chromium nitrate in ethanol and stir by ultrasonic until the mixture is uniform;
[0054] (2) The substrate catalyst RuO2 supported on carbon paper / conductive glass was immersed in the Cr2O3 precursor solution for 1.5
[0055] min and then dried at room temperature.
[0056] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 425°C at a heating rate of 8°C / min, then kept warm for 3.5 h, and then cooled to room temperature in the furnace; thus, a Cr2O3-modified RuO2 catalyst was obtained.
[0057] In the Cr2O3-modified RuO2 catalyst, the atomic percentage of Cr is 12%.
[0058] Example 6: TiO2-modified CoOx Catalyst preparation
[0059] (1) Preparation of TiO2 precursor solution: Use titanium isopropoxide solution as the precursor with a concentration of 0.15 M;
[0060] (2) The substrate catalyst CoO loaded on carbon paper / conductive glass x Immerse in the TiO2 precursor solution for 1 min and then dry at room temperature.
[0061] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 400°C at a heating rate of 10°C / min, then kept at this temperature for 3h, and then cooled to room temperature with the furnace; TiO2-modified CoO x Catalyst. TiO2-CoO x The morphology of the catalysts was characterized by Figure 2 .in, Figure 2 a means scanned image, Figure 2 b indicates transmission image
[0062] TiO2 modified CoO x The atomic percentage of Cr in the catalyst was 10%.
[0063] Example 7: TiO2-modified NiO x Catalyst preparation
[0064] (1) Preparation of TiO2 precursor solution: Use titanium isopropoxide solution as the precursor with a concentration of 0.05 M;
[0065] (2) The substrate catalyst CoO loaded on carbon paper / conductive glass x Immerse in the TiO2 precursor solution for 0.5 min and then dry at room temperature.
[0066] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 400°C at a heating rate of 10°C / min, then kept at this temperature for 3h, and then cooled to room temperature with the furnace; TiO2-modified CoO x catalyst.
[0067] TiO2 modified CoO x The atomic percentage of Ti in the catalyst is 5%.
[0068] Example 8: TiO2-modified MnO x Catalyst preparation
[0069] (1) Preparation of TiO2 precursor solution: Use titanium isopropoxide solution as the precursor with a concentration of 0.05 M;
[0070] (2) The substrate catalyst MnO supported on carbon paper / conductive glass x Immerse in the TiO2 precursor solution for 0.5 min and then dry at room temperature.
[0071] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 400°C at a heating rate of 10°C / min, then kept at this temperature for 3 h, and then cooled to room temperature with the furnace; thus, TiO2-modified MnO x catalyst.
[0072] TiO2 modified MnO x The atomic percentage of Ti in the catalyst is 5%.
[0073] Example 9: Preparation of TiO2-modified Pt catalyst
[0074] (1) Preparation of TiO2 precursor solution: Use titanium isopropoxide solution as the precursor with a concentration of 0.6 M;
[0075] (2) The substrate catalyst Pt supported on carbon paper / conductive glass is immersed in the TiO2 precursor solution for 1.5 min and then dried at room temperature.
[0076] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 375°C at a heating rate of 5°C / min, then kept warm for 2.5 h, and then cooled to room temperature in the furnace; thus, a TiO2-modified Pt catalyst was obtained.
[0077] In the TiO2-modified Pt catalyst, the atomic percentage of Ti is 35%.
[0078] Example 10: Preparation of TiO2-modified RuO2 catalyst
[0079] (1) Preparation of Cr2O3 precursor solution: dissolve 0.25 M chromium nitrate in ethanol and stir by ultrasonic until the mixture is uniform;
[0080] (2) The substrate catalyst RuO2 supported on carbon paper / conductive glass is immersed in the TiO2 precursor solution for 1.5 minutes and then dried at room temperature.
[0081] (3) Annealing: The sample was placed in a vacuum tube furnace and vacuum annealed under nitrogen protection: heated to 425°C at a heating rate of 8°C / min, then kept warm for 3.5 h, and then cooled to room temperature in the furnace; thus, a TiO2-modified RuO2 catalyst was obtained.
[0082] The atomic percentage of Cr in the TiO2-modified RuO2 catalyst is 16%.
[0083] Example 11: Performance test of the catalysts described in Examples 1-8 in a neutral electrolyte
[0084] The hydrogen evolution and oxygen evolution reaction tests were performed using a CHI 660E electrochemical workstation, using the catalysts described in Examples 1-8 as the working electrode, a carbon rod as the counter electrode, and a calomel electrode (SCE) as the reference electrode (E SCE Convert to E RHE The calculation formula is: E RHE =E SCE +0.71V) and conduct three-electrode electrochemical system test.
[0085] a) Hydrogen evolution performance test: The electrolyte is natural seawater saturated with nitrogen (neutral, pH = 7.9), and the nitrogen atmosphere is maintained during the reaction. First, the cyclic voltammetry (CV) curve is tested until it coincides: voltage range: -0.61 ~ (-1.01) VSCE, scan rate: 50mV s -1 ; Then test the polarization curve linear sweep voltammetry (LSV) curve: voltage range: -0.61 ~ (-1.01) V SCE, scan rate: 5mV s -1 ;
[0086] b) Oxygen evolution performance test: The electrolyte is natural seawater saturated with oxygen (neutral, pH = 7.9), and the oxygen atmosphere is maintained during the reaction. First, test the cyclic voltammetry (CV) curve until it coincides: Voltage range: 0.49 ~ 1.29
[0087] VSCE, scan rate: 50 mV s -1 ; Then test the polarization curve linear sweep voltammetry (LSV) curve: voltage range: 0.49 ~ 1.29V SCE, scan rate: 5mV s -1 ;
[0088] Example 12: Performance test results of the catalysts described in Examples 1, 2, 3 and 6 in neutral electrolyte:
[0089] The catalysts described in Examples 1, 2, 3 and 6 are modified by Cr2O3 or TiO2. During the hydrogen and oxygen evolution reactions, the electrode surface forms a local alkaline reaction environment (such as Figure 3 ). Specifically, the local pH change on the anode surface during oxygen evolution is as follows: Figure 3 As shown in a, the pH change of the cathode surface during hydrogen evolution is as follows Figure 3 b. Therefore, the performance of hydrogen and oxygen evolution in neutral electrolyte is greatly improved. x The catalyst exhibits the best hydrogen and oxygen evolution performance (performance curves such as Figure 4As shown. Figure 4 a represents the oxygen evolution performance curve, Figure 4 b represents the hydrogen evolution performance curve): 10mA cm -2 At current density, pure CoO x Compared with the catalyst, Cr2O3-CoO x The overpotentials of hydrogen evolution and oxygen evolution of the catalyst decreased by 0.22 and 0.31 V respectively. The actual overpotential of hydrogen evolution was only 0.10 V; the overpotential of oxygen evolution was only 0.46 V. Example 2 - Cr2O3 modified NiO x , 3-Cr2O3 modified MnO x and 6-TiO2 modified CoO x Catalyst at 10 mA cm -2 The oxygen evolution overpotentials at the current density are 0.56V, 0.72V and 0.47V respectively (the oxygen evolution performance curve is shown in Figure 5 As shown. Figure 5 a represents Cr2O3-NiO x Oxygen evolution performance curve, Figure 5 b represents Cr2O3-MnO x Oxygen evolution performance curve, Figure 5 d represents TiO2-CoO x Oxygen evolution performance curve)
[0090] The technical solutions disclosed and proposed by the present invention can be realized by those skilled in the art by referring to the contents of this article and appropriately changing the conditions, routes and other links. Although the methods and preparation techniques of the present invention have been described through preferred embodiments, relevant technicians can obviously modify or re-combine the methods and technical routes described herein without departing from the content, spirit and scope of the present invention to realize the final preparation technology. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the spirit, scope and content of the present invention.
Claims
1. A method for constructing a catalyst in a local alkaline environment; characterized in that A series of substrate catalysts construct a local alkaline environment on the surface of the substrate catalyst by introducing a hard Lewis acid layer; Lewis acid C r2 O3 or TiO2; in the Lewis acid-modified transition metal oxide catalyst, the atomic percentage of Cr is 2 to 20%; the atomic percentage of Ti is 5 to 35%; The steps include: (1) The Cr2O3 precursor solution is an ethanol solution of chromium nitrate with a concentration of 0.02~0.5 M; The TiO2 precursor solution is titanium isopropoxide solution with a concentration of 0.05~0.6 M; (2) Immerse the substrate catalyst transition metal oxide in the precursor solution for 0.5-1.5 min and then take it out and dry it; (3) The vacuum annealing process was carried out in a vacuum tube furnace under argon / nitrogen protection; the annealing temperature was set at 375~425℃, the rate of rising from room temperature to the set temperature was 5~10℃ / min, and the temperature was kept at this temperature for 2.5~3.5 h; the vacuum degree was less than 3.0×10 -1 Entrust.
2. The catalyst prepared by the method for constructing a catalyst in a local alkaline environment according to claim 1 is applied to the electrocatalytic reaction of hydrogen evolution or oxygen evolution.