A method for preparing high-performance micron-level physical sunscreen
By rutile nanotitanium dioxide as a core body, the nucleation and crystallization of titanium ions are controlled in stages to generate titanium dioxide with micro-nano multi-level structures, the problem of poor ultraviolet shielding effect when the particle size of nanotitanium dioxide is less than 100 nanometers is solved, and the problem of poor ultraviolet shielding effect is achieved Effective shielding of medium and long wave ultraviolet rays and suitable for large-scale production.
Patent Information
- Application Number
- CN202211673229.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-26
AI Technical Summary
The existing nanotitanium dioxide particles have a particle size of less than 100 nanometers, which may cause potential harm to humans. At the same time, their ultraviolet shielding effect is poor, making it difficult to prepare micron-scale titanium dioxide with excellent ultraviolet shielding effect.
Using rutile nanotitanium dioxide as a core body, the nucleation and crystallization rate of titanium ions are controlled through phased temperature increase, titanium ions are induced to crystallize and grow on the surface, and rutile titanium dioxide with micro-nano multi-level structure is generated to prepare high-performance micron-level physical sun protection agent. The specific steps include adding titanium tetrachloride and rutile nanotitanium dioxide at a temperature of 0 to 30°C, adding sodium hydroxide solution, performing phased heating and standing insulation, and finally filtering, washing, drying and pulverizing to obtain micro-nano multi-stage Structural titanium dioxide powder.
It realizes effective shielding of medium and long-wave ultraviolet rays, with gentle process, short process, simple operation, low raw material cost, suitable for large-scale production, and has a good sunscreen index through simulated sunscreen tests.
Smart Images

Figure BDA0004017011320000041 
Figure HDA0004017011330000011 
Figure HDA0004017011330000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic non-metallic functional materials, and in particular relates to a method for preparing a high-performance micron-sized physical sunscreen agent which is formed by agglomerating rutile nano-titanium dioxide into micron-sized large particles. Background Art
[0002] Ultraviolet rays in sunlight can cause serious harm to humans. Among them, medium-wave ultraviolet rays (UVB) with a wavelength of 290 to 320 nm can cause redness, blisters, peeling and inflammation of the skin; long-wave ultraviolet rays (UVA) with a wavelength of 320 to 400 nm can cause skin tanning, aging, skin cancer and DNA damage. Nano titanium dioxide not only has the advantages of non-toxicity, good chemical stability and thermal stability, but also can absorb ultraviolet rays and scatter ultraviolet rays when added to cosmetics. It is a widely used physical sunscreen. Recently, some studies have shown that titanium dioxide particles with a particle size of less than 100 nanometers may cause potential harm to people. When the particle size of titanium dioxide is greater than 100 nanometers, their ultraviolet shielding effect is greatly reduced. Therefore, the preparation of micron-sized titanium dioxide with excellent ultraviolet shielding effect is a key technical problem. Summary of the invention
[0003] In view of the problems existing in the background technology, the purpose of the present invention is to provide a high-performance micron-level physical sunscreen and a preparation method thereof.
[0004] The technical solution adopted by the present invention is as follows:
[0005] A high-performance micron-level physical sunscreen, the preparation method of which is to use rutile nano-titanium dioxide as a core, induce titanium ions to crystallize and grow on its surface, and generate rutile titanium dioxide with a micro-nano multi-level structure, the specific steps are as follows:
[0006] (1) Add rutile nano-titanium dioxide to a titanium tetrachloride aqueous solution having a concentration of 1 to 3 mol / L at a temperature of 0 to 30° C., stir and disperse, and obtain a dispersion slurry.
[0007] (2) Add 1-4 mol / L sodium hydroxide solution to the dispersion slurry obtained in step (1), maintain the system temperature at 0-30° C. After the sodium hydroxide solution is added, stop stirring and let it stand for 3-6 hours.
[0008] (3) First, the temperature is raised to 50-60° C., and the mixture is allowed to stand for 1-3 hours. Then, the temperature is raised to 65-75° C., and the mixture is allowed to stand for 2-4 hours. Finally, the temperature is raised to 85-95° C., and the mixture is stirred for 5-8 hours to generate a rutile titanium dioxide dispersion slurry having a micro-nano multi-level structure.
[0009] (4) The mixed slurry obtained in step (3) is filtered, washed with deionized water, dried, and crushed to obtain rutile titanium dioxide powder with a micro-nano multi-level structure.
[0010] Furthermore, the grain size of the rutile nano-titanium dioxide in step (1) is less than 10 nanometers, and the grain size is calculated by the Scherrer formula based on the X-ray diffraction line broadening method.
[0011] Furthermore, the amount of rutile nano-titanium dioxide used in step (1) is calculated based on the molar number of titanium tetrachloride added, and the molar ratio of rutile nano-titanium dioxide to titanium tetrachloride is 1:5-30.
[0012] Furthermore, the amount of the sodium hydroxide aqueous solution in step (2) is calculated based on the molar number of titanium tetrachloride added, and the molar ratio of sodium hydroxide to titanium tetrachloride is 1.5 to 3:1.
[0013] Beneficial effects of the present invention: The method of the present invention uses rutile nano-titanium dioxide as a core body, controls the nucleation and crystallization rate of titanium ions by staged temperature increase, induces titanium ions to crystallize and grow on its surface, and generates rutile titanium dioxide with a micro-nano multi-level structure. The process conditions of the present invention are mild, the process is short, the operation is simple, the raw material cost is low and it is easy to obtain, and it is very suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a TEM photo of the product obtained in Example 1;
[0015] Figure 2 This is a TEM photo of the product obtained in Example 2;
[0016] Figure 3 This is a TEM photo of the product obtained in Example 3;
[0017] Figure 4 The following are the X-ray diffraction patterns of the products obtained in Examples 1 to 3. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below in conjunction with embodiments: These embodiments are only used to illustrate the present invention and are not used to limit the scope of the invention.
[0019] Example 1
[0020] (1) At a temperature of 0° C., 2 mol of rutile nano-titanium dioxide with a crystal size of 6.8 nanometers was added to 10 liters of titanium tetrachloride aqueous solution with a concentration of 1 mol / L, and the mixture was stirred and dispersed to obtain a dispersion slurry.
[0021] (2) Add 15 liters of 1 mol / L sodium hydroxide solution to the dispersion slurry obtained in step (1), maintain the system temperature at 0°C, stop stirring after the sodium hydroxide solution is added, and let it stand and keep warm for 6 hours.
[0022] (3) First, the temperature is raised to 50°C, and the mixture is kept at a temperature of 1 hour. Then, the temperature is raised to 65°C, and the mixture is kept at a temperature of 4 hours. Finally, the temperature is raised to 85°C, and the mixture is kept at a temperature of 5 hours to generate a rutile titanium dioxide dispersion slurry having a micro-nano multi-level structure.
[0023] (4) The mixed slurry obtained in step (3) is filtered, washed with deionized water, dried, and crushed to obtain rutile titanium dioxide powder with a micro-nano multi-level structure.
[0024] Example 2
[0025] (1) At a temperature of 30° C., 1 mol of rutile nano-titanium dioxide with a crystal size of 6.8 nanometers was added to 10 liters of titanium tetrachloride aqueous solution with a concentration of 3 mol / L, and the mixture was stirred and dispersed to obtain a dispersion slurry.
[0026] (2) Add 22.5 liters of 4 mol / L sodium hydroxide solution to the dispersion slurry obtained in step (1), maintain the system temperature at 30° C. After the sodium hydroxide solution is added, stop stirring and let it stand for 3 hours.
[0027] (3) First, the temperature is raised to 60°C, and the mixture is kept at a temperature of 3 hours. Then, the temperature is raised to 75°C, and the mixture is kept at a temperature of 2 hours. Finally, the temperature is raised to 95°C, and the mixture is kept at a temperature of 8 hours to generate a rutile titanium dioxide dispersion slurry having a micro-nano multi-level structure.
[0028] (4) The mixed slurry obtained in step (3) is filtered, washed with deionized water, dried, and crushed to obtain rutile titanium dioxide powder with a micro-nano multi-level structure.
[0029] Example 3
[0030] (1) At a temperature of 20° C., 2 mol of rutile nano-titanium dioxide with a crystal size of 6.8 nanometers was added to 10 liters of a 2 mol / L titanium tetrachloride aqueous solution, and the mixture was stirred and dispersed to obtain a dispersion slurry.
[0031] (2) Add 22 liters of 2 mol / L sodium hydroxide solution to the dispersion slurry obtained in step (1), maintain the system temperature at 20° C. After the sodium hydroxide solution is added, stop stirring and let it stand for 5 hours.
[0032] (3) First, the temperature is raised to 55°C, and the mixture is kept at a temperature of 2 hours. Then, the temperature is raised to 70°C, and the mixture is kept at a temperature of 3 hours. Finally, the temperature is raised to 90°C, and the mixture is kept at a temperature of 7 hours to generate a rutile titanium dioxide dispersion slurry having a micro-nano multi-level structure.
[0033] (4) The mixed slurry obtained in step (3) is filtered, washed with deionized water, dried, and crushed to obtain rutile titanium dioxide powder with a micro-nano multi-level structure.
[0034] Simulate sunscreen sun protection factor test
[0035] The sunscreen performance analyzer (UV-2000S, Lanfei Company, USA) was used to analyze and test the sun protection index of the prepared composite material. 0.2g sample (sunscreen) and 1.8g vaseline were ground evenly in a mortar until there was no particle, which was used as a simulated sunscreen. According to the Colipa standard, 32.5mg of sunscreen was accurately weighed and evenly dispersed on a clean PMMA board. The sunscreen was evenly applied to the entire sample board using a latex finger cot, and the SPF value and PFA value of the sample were tested. The SPF value reflects the protective effect against medium-wave ultraviolet rays (UVB), and the PFA value reflects the protective effect against long-wave ultraviolet rays (UVA). The larger the value, the better the protective effect. As can be seen from Table 1, this product has a good shielding effect on long-wave ultraviolet rays (UVA) and medium-wave ultraviolet rays (UVB).
[0036] Table 1 Comparison of UV shielding effects of different products
[0037]
Claims
1. A method for preparing a high-performance micron-level physical sunscreen agent, It is characterized in that Taking rutile nano-titanium dioxide as the core, inducing titanium ions to crystallize and grow on its surface to generate rutile titanium dioxide with a micro-nano multi-level structure; specifically comprising the following steps: (1) adding rutile nano-titanium dioxide to a titanium tetrachloride aqueous solution at a temperature of 0 to 30°C, stirring to disperse the mixture uniformly, and obtaining a dispersion slurry; the grain size of the rutile nano-titanium dioxide is less than 10 nanometers; the amount of the rutile nano-titanium dioxide is calculated based on the molar number of titanium tetrachloride added, and the molar ratio of the rutile nano-titanium dioxide to the titanium tetrachloride is 1:5 to 30; (2) adding sodium hydroxide solution to the dispersion slurry obtained in step (1); after the sodium hydroxide solution is added, stopping stirring and standing to keep warm for 3 to 6 hours; the amount of the sodium hydroxide solution is calculated based on the molar number of titanium tetrachloride added, and the molar ratio of sodium hydroxide to titanium tetrachloride is 1.5 to 3:1; the stirring and heat preservation system temperature is maintained at 0 to 30°C; (3) heating the dispersion slurry of step (2) in stages to generate a rutile titanium dioxide dispersion slurry having a micro-nano multi-level structure; the staged heating is: firstly heating to 50-60°C, standing and keeping warm for 1-3 hours; then heating to 65-75°C, standing and keeping warm for 2-4 hours; finally heating to 85-95°C, keeping warm and stirring for 5-8 hours; (4) The mixed slurry obtained in step (3) is filtered, washed with deionized water, dried, and crushed to obtain rutile titanium dioxide powder with a micro-nano hierarchical structure.
2. The method for preparing the high-performance micron-sized physical sunscreen according to claim 1, It is characterized in that The concentration of the titanium tetrachloride aqueous solution in step (1) is 1 to 3 mol / L.
3. The method for preparing the high-performance micron-sized physical sunscreen according to claim 1, It is characterized in that The concentration of the sodium hydroxide solution in step (2) is 1 to 4 mol / L.