A UV-moisture-cured aging-resistant organic silicon pressure-sensitive adhesive material and preparation method thereof
Through UV-moisture dual curing technology, combined with components such as hydroxyl end-embedded modified amino silicone rubber and MQ silicone resin, the shadow area and resistance problems of UV photocuring silicone pressure-sensitive adhesive during the photocuring process are solved, achieving high Coating material with cross-linking, strong bonding properties and aging resistance.
Patent Information
- Application Number
- CN202211548549.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-05
AI Technical Summary
UV photocuring silicone pressure-sensitive adhesive has a shadowed area during the photocuring process, which affects the conversion rate of the photocuring group. The solvent resistance and aging resistance of the coating are affected by the degree of cross-linking, and the cohesion force is small and cannot be continuously adhered to. The surface of the bonded substrate.
UV-moisture dual curing technology is adopted to introduce hydroxyl-terminated acrylate modified amino silicone rubber and hydroxyl-terminated silicone phosphate modified amino silicone rubber into silicone pressure-sensitive adhesive, and with MQ silicone resin and silicone The components such as tackifier and catalyst are mixed and cured by UV light and heating.
The crosslinking degree of silicone pressure-sensitive adhesive is improved, its adhesive properties, solvent resistance and aging resistance are enhanced, the problem of shadowed areas during photocuring is solved, and the continuous adhesion ability of the coating is improved.
Smart Images

Figure FDA0005096876160000011 
Figure FDA0005096876160000012 
Figure GDA0005076760750000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic silicon pressure-sensitive adhesives, and in particular relates to a UV-moisture-cured, aging-resistant organic silicon pressure-sensitive adhesive material and a preparation method thereof. Background Art
[0002] UV light-curing silicone pressure-sensitive adhesive has many unique properties, such as heat resistance, weather resistance, aging resistance, acid and alkali resistance, water repellency, solvent resistance, etc. These excellent properties are unmatched and cannot be replaced by other organic polymer pressure-sensitive adhesives. Therefore, UV light-curing silicone pressure-sensitive adhesive has been widely used in aerospace, electronics and electrical, chemical textile, medical and health, mechanical construction and other fields. However, during the photocuring process of UV light-curing silicone pressure-sensitive adhesive, there is a shadow area in the coating, which affects the conversion rate of the photocuring group of the silicone pressure-sensitive adhesive. The solvent resistance and aging resistance of the silicone pressure-sensitive adhesive coating are affected by the degree of crosslinking. In addition, the cohesive force of the silicone coating is very small and cannot be continuously adhered to the surface of the bonded substrate. These have greatly limited the application of silicone pressure-sensitive adhesive coatings. At present, the most effective method is to graft the silicone pressure-sensitive adhesive containing acrylate, the surface energy of acrylate is 59-67mN / m, and the surface energy is much greater than that of silicone resin. And by introducing a double cross-linking mechanism, a silicone pressure-sensitive adhesive with a high degree of cross-linking, strong bonding performance, solvent resistance and aging resistance can be obtained, making the silicone pressure-sensitive adhesive applicable to more fields.
[0003] At present, the companies producing silicone pressure-sensitive adhesives mainly include: Dow Corning of the United States, Shin-Etsu of Japan, Dow of the United States, Momentive, Wacker of Germany, etc. However, these companies all produce silicone pressure-sensitive adhesives by dissolving prepolymers in toluene and then applying them and heating to evaporate the solvent, which requires the use of a large amount of organic solvents. The prepared polymers are prone to residual solvents and odors, and the scope of application is limited. Summary of the invention
[0004] In order to solve the problems in the related art, the present application provides a UV-moisture-cured aging-resistant silicone pressure-sensitive adhesive material and a preparation method thereof, which solves the problem of low crosslinking degree in a single curing process of UV light-cured silicone pressure-sensitive adhesive.
[0005] The technical solution is as follows:
[0006] A UV-moisture-cured, aging-resistant silicone pressure-sensitive adhesive material, the pre-cured structure of the silicone pressure-sensitive adhesive is as follows:
[0007]
[0008] in:
[0009] m=100~500, n=100~500, x=0~100;
[0010] R1 is dimethylphenylsilyl SiPh(CH3)2 or trimethylsilyl Si(CH3)3;
[0011] R2 is dimethylvinylsilyl SiCH=CH2(CH3)2;
[0012] Rx is one of C2 H4 NHC2 H4 NH(H2 PO4), C2 H4 NHC2 H4 N(H2 PO4)2, C2 H4 NHC2 H4N(HPO4), C2 H4 N(H2 PO4)C2 H4 NH(H2 PO4), C2 H4 N(H2 PO4)C2 H4 N(H2 PO4)2 and C2 H4N(H2 PO4)C2 H4 N(HPO4).
[0013] Furthermore, the formula components of the silicone pressure-sensitive adhesive material include: 20-40 parts of hydroxyl-terminated acrylate modified amino silicone rubber, 20-40 parts of hydroxyl-terminated silicon-based phosphate modified amino silicone rubber, 30-60 parts of MQ silicone resin, 1-5 parts of silicone tackifier, 1-5 parts of silicone leveling agent, 10.1-1 parts of catalyst, 20.1-1 parts of catalyst, and 0.1-1 parts of photoinitiator.
[0014] Further, the structure of the hydroxyl-terminated acrylate modified amino silicone rubber is as follows:
[0015]
[0016] Among them, m=100-500, and the molecular weight of the chain segment is 60000-300000.
[0017] Further, the hydroxyl-terminated silicon-based phosphate modified amino silicone rubber is synthesized from monomers, and the polymer structure is as follows:
[0018]
[0019] in,
[0020] Rx is one of C2 H4 NHC2 H4 NH(H2 PO4), C2 H4 NHC2 H4 N(H2 PO4)2, C2 H4 NHC2 H4N(HPO4), C2 H4 N(H2 PO4)C2 H4 NH(H2 PO4), C2 H4 N(H2 PO4)C2 H4 N(H2 PO4)2 and C2 H4N(H2 PO4)C2 H4 N(HPO4);
[0021] n=100-500, and the chain segment molecular weight is 10000-100000.
[0022] Furthermore, the MQ silicone resin is prepared by hydrolysis and polycondensation reaction of tetraethoxysilane monomer, tetramethyldisiloxane containing phenyl and vinyl groups, and hexamethyldisiloxane.
[0023] Furthermore, the hydroxyl-terminated acrylate-modified amino silicone rubber and the hydroxyl-terminated silyl phosphate-modified amino silicone rubber are synthesized from monomers, and the structure of the monomers is
[0024] wait,
[0025] n=3-6, R is an alkyl group, a phenyl group, etc., and RA is an alkyl group, an N-(β-aminoethyl-γ-aminopropyl) group, a phenyl group, etc.
[0026] Furthermore, the organosilicon tackifier is hydroxyethyl methacrylate, hydroxypropyl methacrylate, methacrylic acid, hexyl methacrylate isocyanate, or glycidyl methacrylate.
[0027] Furthermore, the organosilicon leveling agent is one or two of amino silicone oil, phenyl silicone oil and hydroxy silicone oil.
[0028] Further, the catalyst 1 is an alkaline catalyst or an acidic catalyst, which can be solid, liquid, etc. Specifically, it is one of potassium hydroxide, sodium hydroxide, aluminum hydroxide, tetramethylammonium hydroxide, sulfuric acid, phosphoric acid, ammonium hydrogen phosphate, trifluorosulfonic acid, p-hydroxybenzoic acid, and solid acid.
[0029] Furthermore, the catalyst 2 is an organic bismuth catalyst, specifically one or two of bismuth octanoate, bismuth laurate, bismuth cyclohexaneate, bismuth oxide, and bismuth nitrate.
[0030] Further, the photoinitiator is one or two of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and methyl benzoylformate.
[0031] A method for preparing a UV-moisture-cured, aging-resistant organic silicon pressure-sensitive adhesive material, the preparation method is as follows:
[0032] After mixing the organosilicon monomer, organosilicon ring body and catalyst 1 in a certain proportion, add them into a reactor, protect with nitrogen, heat up to 40-120°C, react for 2-8h, add phosphoric acid or glycidyl methacrylate, cool to 40-80°C, react for 4-10h, cool down, neutralize, filter and remove low-boiling substances to obtain viscous hydroxyl-terminated acrylate-modified amino silicone rubber and hydroxyl-terminated silicon-based phosphate-modified amino silicone rubber.
[0033] Tetraethoxysilane monomer, ethoxysilane containing phenyl and vinyl monomers, and hexamethyldisiloxane are mixed in a certain proportion, added into a reaction kettle, heated to 40-120° C., catalyst 1 is added, reacted for 2-8 hours, extracted, and a viscous MQ silicone resin is obtained.
[0034] The hydroxyl-terminated acrylate-modified amino silicone rubber and the hydroxyl-terminated silicon-based phosphate-modified amino silicone rubber are uniformly mixed with MQ silicone resin, silicone leveling agent, silicone tackifier, catalyst 2, and photoinitiator, and then cured under UV light conditions and heating conditions to obtain an aging-resistant silicone coating material.
[0035] It is to be understood that the foregoing general description and the following detailed description are exemplary only and are not restrictive of the invention. DETAILED DESCRIPTION
[0036] The embodiments of the present invention include:
[0037] Example 1
[0038] 100 parts of octamethylcyclotetrasiloxane, 10 parts of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane, and 0.1 parts of KOH catalyst were mixed evenly and added to a 500mL reactor. The mixture was heated to 70°C under nitrogen protection, reacted for 8 hours, cooled to 45°C, neutralized with 20 parts of phosphoric acid or glycidyl acrylate, reacted for 4 hours, cooled, filtered, and vacuumed to remove low-boiling substances to obtain hydroxyl-terminated acrylate-modified aminosilicone rubber or hydroxyl-terminated silyl phosphate-modified aminosilicone rubber. 100 parts of tetraethoxysilane monomer, 10 parts of diphenyltetramethyldisiloxane, 10 parts of divinyltetramethyldisiloxane, and 10 parts of hexamethyldisiloxane were mixed in a certain proportion, added to a reactor, heated to 40-120°C, 1g of hydrochloric acid was added, reacted for 2-8 hours, and extracted to obtain a viscous MQ silicone resin.
[0039] 20 parts of hydroxyl-terminated acrylate modified amino silicone rubber and 20 parts of hydroxyl-terminated silicon-based phosphate modified amino silicone rubber, 60 parts of MQ silicone resin, 1 part of hydroxyl silicone oil, 1 part of methacrylic acid, 0.1 parts of bismuth octanoate and 1 part of 2-hydroxy-2-methyl-1-phenylacetone were uniformly mixed, and then cured under UV light and heating conditions to obtain a UV-moisture dual-curing aging-resistant silicone pressure-sensitive adhesive.
[0040] Example 2
[0041] The prepolymer preparation process is the same as in Example 1
[0042] 20 parts of hydroxyl-terminated acrylate modified amino silicone rubber, 40 parts of hydroxyl-terminated silicon-based phosphate modified amino silicone rubber, 60 parts of MQ silicone resin, 1 part of hydroxyl silicone oil, 1 part of methacrylic acid, 0.1 parts of bismuth octanoate and 0.1 parts of 2-hydroxy-2-methyl-1-phenylpropanone were uniformly mixed, and then cured under UV light and heating conditions to obtain a UV-moisture dual-curing aging-resistant silicone pressure-sensitive adhesive.
[0043] Example 3
[0044] The prepolymer preparation process is the same as in Example 1
[0045] 40 parts of hydroxyl-terminated acrylate modified amino silicone rubber and 40 parts of hydroxyl-terminated silicon-based phosphate modified amino silicone rubber, 60 parts of MQ silicone resin, 1 part of hydroxyl silicone oil, 1 part of methacrylic acid, 0.1 parts of bismuth octanoate and 0.1 parts of 2-hydroxy-2-methyl-1-phenylpropanone were uniformly mixed, and then cured under UV light and heating conditions to obtain a UV-moisture dual-curing aging-resistant silicone pressure-sensitive adhesive.
[0046] Example 4
[0047] The prepolymer preparation process is the same as in Example 1
[0048] 40 parts of hydroxyl-terminated acrylate-modified amino silicone rubber and 40 parts of hydroxyl-terminated silyl phosphate-modified amino silicone rubber were mixed with 30 parts of MQ silicone resin, 1 part of hydroxyl silicone oil, 1 part of methacrylic acid, 0.1 parts of bismuth octanoate, 0.1 parts of 2-hydroxy-2-
[0049] After the methyl-1-phenylacetone is evenly mixed, the mixture is cured under UV light conditions and heating conditions to obtain a UV-moisture dual-curing aging-resistant silicone pressure-sensitive adhesive.
[0050] Example 5
[0051] The prepolymer preparation process is the same as in Example 1
[0052] 20 parts of hydroxyl-terminated acrylate-modified amino silicone rubber and 20 parts of hydroxyl-terminated silicon-based phosphate-modified amino silicone rubber, 60 parts of MQ silicone resin, 2.5 parts of hydroxyl silicone oil, 2.5 parts of methacrylic acid, 0.5 parts of bismuth octanoate and 0.5 parts of 2-hydroxy-2-methyl-1-phenylpropanone were uniformly mixed, and then cured under UV light and heating conditions to obtain a UV-moisture dual-curing aging-resistant silicone pressure-sensitive adhesive.
[0053] Example 6
[0054] The prepolymer preparation process is the same as in Example 1
[0055] 20 parts of hydroxyl-terminated acrylate modified amino silicone rubber and 20 parts of hydroxyl-terminated silicon-based phosphate modified amino silicone rubber, 60 parts of MQ silicone resin, 5 parts of hydroxyl silicone oil, 5 parts of methacrylic acid, 1 part of bismuth octanoate and 1 part of 2-hydroxy-2-methyl-1-phenylacetone were uniformly mixed, and then cured under UV light and heating conditions to obtain a UV-moisture dual-curing aging-resistant silicone pressure-sensitive adhesive.
[0056] Test standards: Peel force test standard: GB 2792-1998; Stickiness test standard: GB / T 4851-2014; Initial adhesion test standard: GB / T 31125-2014; Alkali resistance test standard: GB / T 9265-2009; Acid resistance test standard: GB / T1733-1993; Salt spray resistance test standard GB10125-1997.
[0057] The test results are as follows:
[0058]
[0059] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention invented herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not invented by the present invention. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present invention are indicated by the appended claims.
[0060] It should be understood that the present invention is not limited to the precise construction that has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A UV-moisture curing aging-resistant organic silicone pressure-sensitive adhesive material, characterized in that: The formula components of the organic silicon pressure-sensitive adhesive material include: 20-40 parts of hydroxyl-terminated acrylate modified amino silicone rubber, 20-40 parts of hydroxyl-terminated silicon-based phosphate modified amino silicone rubber, 30-60 parts of MQ silicone resin, 1-5 parts of organic silicon tackifier, 1-5 parts of organic silicon leveling agent, 0.1-1 parts of catalyst 1, 0.1-1 parts of catalyst 2, and 0.1-1 parts of photoinitiator; The preparation method of the hydroxyl-terminated acrylate-modified aminosilicone rubber and the hydroxyl-terminated silyl phosphate-modified aminosilicone rubber is as follows: after mixing an organosilicon monomer, an organosilicon ring body and a catalyst 1 in a certain proportion, adding the mixture into a reaction kettle, protecting with nitrogen, heating to 40-120° C., reacting for 2-8 hours, adding phosphoric acid or glycidyl methacrylate, cooling to 40-80° C., reacting for 4-10 hours, cooling, neutralizing, filtering and removing low-boiling substances, and obtaining viscous hydroxyl-terminated silyl phosphate-modified aminosilicone rubber and hydroxyl-terminated acrylate-modified aminosilicone rubber; Wherein, the structure of the organosilicon monomer is: R A is an N-(β-aminoethyl-γ-aminopropyl) group; The structure of the organosilicon ring is: n=3-6, R is alkyl or phenyl; The MQ silicone resin is prepared by hydrolysis and polycondensation reaction of tetraethoxysilane monomer, tetramethyldisiloxane containing phenyl, tetramethyldisiloxane containing vinyl, and hexamethyldisiloxane; The organosilicon tackifier is hydroxyethyl methacrylate, hydroxypropyl methacrylate, methacrylic acid, hexyl methacrylate isocyanate, and glycidyl methacrylate; The organosilicon leveling agent is one or two of amino silicone oil, phenyl silicone oil and hydroxy silicone oil; The catalyst 1 is an alkaline catalyst or an acidic catalyst; specifically, one of potassium hydroxide, sodium hydroxide, aluminum hydroxide, tetramethylammonium hydroxide, sulfuric acid, phosphoric acid, ammonium hydrogen phosphate, trifluorosulfonic acid, and p-hydroxybenzoic acid; The catalyst 2 is an organic bismuth catalyst, specifically one or two of bismuth octanoate, bismuth laurate, bismuth cyclohexaneate, bismuth oxide, and bismuth nitrate; The photoinitiator is one or two of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone and methyl benzoylformate.
2. A method for preparing the UV-moisture curing aging-resistant organic silicon pressure-sensitive adhesive material as claimed in claim 1, characterized in that: The preparation method is as follows: after mixing the organosilicon monomer, organosilicon ring body and catalyst 1 in a certain proportion, add them into a reaction kettle, protect with nitrogen, heat up to 40-120°C, react for 2-8h, add phosphoric acid or glycidyl methacrylate, cool down to 40-80°C, react for 4-10h, cool down, neutralize, filter and remove low-boiling substances to obtain viscous hydroxyl-terminated acrylate-modified aminosilicone rubber and hydroxyl-terminated silicon-based phosphate-modified aminosilicone rubber; tetramethyldisiloxane containing phenyl and tetramethyldisiloxane containing vinyl are added. After mixing oxane and hexamethyldisiloxane in a certain proportion, add them into a reactor, heat to 40-120°C, add catalyst 1, react for 2-8h, extract and obtain viscous MQ silicone resin; after uniformly mixing hydroxyl-terminated silyl phosphate-modified amino silicone rubber and hydroxyl-terminated acrylate-modified amino silicone rubber with MQ silicone resin, silicone leveling agent, silicone tackifier, catalyst 2 and photoinitiator, cure under UV light conditions and heating conditions to obtain UV-moisture-cured aging-resistant silicone pressure-sensitive adhesive material.
Citation Information
Patent Citations
Dual curing coating method for substrates with shadow areas
CA1251596A
Polysiloxane with UV (Ultraviolet) and moisture double curing groups and preparation method thereof
CN103923321A
Dual-curing organic silicon resin and preparation method therefor
CN110790936A
Reaction type polyurethane hot melt adhesive with multiple curing modes and preparation method of reaction type polyurethane hot melt adhesive
CN112724915A
Vulcanisable silicone compositions
CN114008167A