A heat treatment process for high-strength alloy camshaft
By using 50CrMoA alloy steel and employing a quenching and tempering heat treatment process, the problems of insufficient hardened layer and easy peeling of existing camshafts have been solved, resulting in a high-strength and wear-resistant camshaft suitable for high-power internal combustion engines, with high and stable processing efficiency.
Patent Information
- Application Number
- CN202211666001.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-23
AI Technical Summary
In the existing technology, the hardened layer depth of camshafts made of 20 steel, 20Cr, and 20Mn2 is insufficient after quenching. The hardened layer of 45 steel and 50 steel camshafts is prone to peeling off in high-power diesel engines. The heat treatment process of Gr15 steel is complicated and prone to grinding cracks, which cannot meet the mechanical and wear resistance requirements of high-power internal combustion engines for camshafts.
Using 50CrMoA alloy steel as the base material, a quenching and tempering heat treatment process is adopted. The quenching temperature is 860℃ and held, and the tempering temperature is 650℃. Combined with multiple preheating cycle scanning heating and spray ring quenching, a uniform hardened layer is obtained with a surface hardness greater than 58HRC and a hardened layer thickness of 4.5-7mm.
It achieves high strength and wear resistance in camshafts, avoids quenching cracks, meets the service life and processing requirements of high-power internal combustion engines, has high processing efficiency, and is suitable for large-scale production.
Smart Images

Figure CN116024423B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of internal combustion engine parts processing, in particular to a high-strength alloy camshaft heat treatment process. Background Art
[0002] The camshaft of a high-power internal combustion engine is an important structural component of a diesel engine. Its function is to control the opening and closing of the valve. When the camshaft rotates at high speed, the cam surface is subjected to cyclic stress and wear occurs, which may cause the surface layer to fall off in severe cases.
[0003] The maximum hardened layer depth of 20 steel, 20Cr, 20Mn2 camshafts specified in the industry standard after carburizing quenching or carbonitriding quenching is 1.5mm, which is less than the lower limit of 3.0mm required by the drawings; 45 steel and 50 steel camshafts are easy to peel off after long-term operation on high-power diesel engines after medium-frequency quenching; Gr15 steel camshafts have complex heat treatment processes, and are prone to grinding cracks after medium-frequency grinding, making them difficult to process. The above materials do not meet the requirements of high-power internal combustion engines for camshaft process performance or performance.
[0004] The inventors found that 50 steel is currently used to produce camshafts for high-power internal combustion engines, and an uneven hardened layer is obtained on the special-shaped cam through normalizing and medium-frequency quenching. However, after the 50 steel camshaft is medium-frequency quenched and operated for a long time on a high-power diesel engine, the hardened layer is easy to peel off, which cannot meet the special requirements of high-power internal combustion engines for the mechanical properties and wear resistance of the camshaft. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high-strength alloy camshaft heat treatment process. When the workpiece is quenched and tempered, the quenching heating temperature is 860°C and the temperature is kept, so that the matrix structure can be completely austenitized and the tensile strength can be improved. At the same time, the workpiece enters the tempering furnace for tempering, the tempering temperature is 650°C, and the workpiece is cooled by water after being kept warm. This can not only obtain better performance, but also avoid the occurrence of the second type of temper brittleness.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A high-strength alloy camshaft heat treatment process comprises the following steps:
[0008] For quenching and tempering heat treatment, the workpiece is placed in a heating furnace, heated to 860℃±10 and kept warm, cooled in a cooling medium, and then sent to a cleaning machine to clean the oil stains; then sent to a tempering furnace for tempering, the tempering temperature is 650℃±10, and then taken out of the furnace for water cooling after keeping warm;
[0009] After the workpiece is tempered and finely machined, it is subjected to medium frequency quenching. The workpiece is placed on a quenching machine and a profile sensor is installed. The workpiece is subjected to multiple preheating cycle scanning heating to obtain a uniform hardened layer. After that, a spray ring quenching cooling is used. The surface hardness of the workpiece is greater than 58HRC, and the hardened layer is 4.5-7mm.
[0010] As a further implementation method, the heating furnace uses the Aixilin multi-purpose furnace production line, model VKEs4 / 2.
[0011] As a further implementation method, the workpiece is placed in a heating furnace, heated to 860°C±10 and kept warm for 3 hours, and the cooling medium is Houghton HQG rapid quenching oil, and cooled for 30 minutes.
[0012] As a further implementation method, when the workpiece enters the tempering furnace for tempering, nitrogen is introduced into the tempering furnace to prevent the workpiece from oxidation, and after keeping the workpiece warm for 3 hours, it enters the cleaning machine for rapid cooling.
[0013] As a further implementation method, the medium frequency quenching uses an EFD vertical induction quenching machine. First, the profiling sensor is placed close to the base circle of the workpiece for preheating, so that the average temperature of the base circle is slightly higher than the temperature of the cam lobe tip and wait for 5-10 seconds;
[0014] The profile sensor then returns to its initial position, performs cyclic scanning heating, and then quenches.
[0015] As a further implementation, when the workpiece is cooled, the bottom cooperates with the base to rotate so that the cooling process is uniform.
[0016] As a further implementation, the spray circle includes an upper auxiliary spray area and a lower main spray area, the main spray flow rate is 90L / min, and the auxiliary spray flow rate is 50L / min.
[0017] As a further implementation method, the first-stage preheating power of the profiling sensor is 90KW, the second-stage cycle scanning heating power is 135Kw, and the sensor moving speed is 260mm / min.
[0018] As a further implementation, the medium frequency current frequency is 7000HZ.
[0019] As a further implementation method, during medium frequency quenching, the intake cam is on top and the exhaust cam is on the bottom.
[0020] The beneficial effects of the present invention are as follows:
[0021] 1. When the workpiece is quenched and tempered by the present invention, the quenching heating temperature is 860℃±10 and the temperature is kept, which can make the matrix structure completely austenitized and improve the tensile strength. At the same time, the workpiece enters the tempering furnace for tempering, the tempering temperature is 650℃±10, and after the temperature is kept, it is cooled by water after being taken out of the furnace, which can not only obtain better performance, but also avoid the occurrence of the second type of temper brittleness.
[0022] 2. The present invention performs medium frequency quenching after fine machining after tempering, and the surface is not affected by oxide scale, and only fine grinding is required after medium frequency to complete the finished product processing, and the processing efficiency and accuracy are guaranteed.
[0023] 3. The quality of the high-power internal combustion engine camshaft produced by this method is stable, with a base hardness of 28-32HRC, a surface hardness of more than 58HRC, a hardened layer of 4.5-7mm, and a uniform distribution, which can meet the special requirements of high-power internal combustion engines for the mechanical properties and wear resistance of the camshaft; no quenching cracking has occurred for two years, the service life is long, and the processing process is relatively simple, which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0025] Figure 1 This is a finishing diagram of the camshaft before medium frequency quenching in an embodiment of the present invention.
[0026] Figure 2 yes Figure 1 Schematic diagram of the shape of the intake cam in the AA direction.
[0027] Figure 3 yes Figure 1 Schematic diagram of the exhaust cam shape in the AA direction.
[0028] Figure 4 1 is a schematic diagram of low-power cyclic scanning preheating in the first stage in an embodiment of the present invention.
[0029] Figure 5 Schematic diagram of high-power scanning heating in the second stage of the embodiment of the present invention.
[0030] In the figure: the distances or sizes between parts are exaggerated to show the positions of various parts, and the schematic diagram is for reference only. DETAILED DESCRIPTION
[0031] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0032] The camshaft of a high-power internal combustion engine is an important structural component of a diesel engine. Its function is to control the opening and closing of the valve. When the camshaft rotates at high speed, the cam surface is subjected to cyclic stress and wear occurs. In severe cases, the surface layer may fall off. The part body is required to have high wear resistance and mechanical properties. The main technical requirements are shown in the table below.
[0033] Cam tip hardness (HRC) Cam base circle hardness (HRC) Hardened layer depth (mm) Surface hardness of substrate 58-64 ≥55 3-8 28-32
[0034] According to the relevant provisions of the mechanical industry standard GB / T 6728.1--201X "Internal Combustion Engine Camshaft Part 1: Technical Conditions", the maximum hardened layer depth of 20 steel, 20Cr, 20Mn2 and other camshafts specified in the standard after carburizing quenching or carbonitriding quenching is 1.5mm, which is less than the lower limit of 3.0mm required by the drawings; 45 steel and 50 steel camshafts are easy to peel off after long-term operation on high-power diesel engines after medium-frequency quenching; Gr15 steel camshafts have complex heat treatment processes, and are prone to grinding cracks after medium-frequency grinding, making them difficult to process. The above materials do not meet the requirements of high-power internal combustion engines for camshaft process performance or performance.
[0035] The current plan is to use 50 steel to produce high-power internal combustion engine camshafts, and obtain an uneven hardened layer on the special-shaped cams through normalizing and medium-frequency quenching.
[0036] In order to meet the special requirements of high-power internal combustion engines for the mechanical properties and wear resistance of camshafts, it is necessary to study a new type of alloy steel camshaft, which can be met through simple tempering and medium-frequency quenching.
[0037] First, optimize the camshaft base material: To solve the problem of camshaft surface peeling, the existing camshaft material is changed from ordinary 50# steel to 50CrMoA. 50CrMoA is high-quality 50CrMo steel with less impurities such as S and P (sulfur and phosphorus), smaller fluctuation range of main components, and more stable quality. By optimizing the alloy steel composition and metallographic structure, the new 50CrMoA alloy steel is used to produce high-power internal combustion engine camshafts, and a relatively uniform hardened layer is obtained on the special-shaped cam through quenching and tempering and medium-frequency quenching to improve fatigue life. Based on the requirements of GB / T3077-2015 standard for 50CrMoA, the requirements for material composition are as follows:
[0038] C Si Mn Cr Mo 0.50~0.54 <0.40 0.50~0.80 0.90~1.20 0.15~0.30
[0039] Secondly, the grain size of the blank is ≥ level 5, the ingot-shaped segregation, central porosity and general porosity level in the acid-etched macrostructure is not greater than level 2, general point segregation and edge point segregation are not allowed, the ultrasonic flaw detection method is in accordance with CB / T3907, the initial sensitivity of ultrasonic flaw detection is ∮2mm equivalent, defects not greater than ∮2mm equivalent are allowed, and intensive defects are not allowed.
[0040] In a typical embodiment of the present invention, reference is made to Figure 1-Figure 5 As shown, a high-strength alloy camshaft heat treatment process comprises the following steps:
[0041] The workpiece is subjected to quenching and tempering heat treatment. Rough machining is required before quenching and tempering. The workpiece is placed in a heating furnace for heating and quenching. The quenching heating temperature is 860℃±10 and kept warm for 3h, preferably 860℃. During rough machining: the parts are manually loaded into the basket, and then the basket is hoisted onto the guide rail. The operator operates the material cart to send the basket into the multi-purpose furnace, and then it automatically runs according to the selected process to remove the oxide layer. When it is out of the furnace, the operator operates the material cart to pull the basket out of the furnace.
[0042] Specifically, the heating furnace uses the Aixilin multi-purpose furnace production line, model VKEs4 / 2. After the furnace is loaded, it is fully automatic. The heating and cooling processes do not require manual intervention, and there is a reducing atmosphere in the furnace to avoid oxidation and decarburization on the workpiece surface.
[0043] The camshaft is suitable for high-power diesel engines with a cylinder diameter of 270mm. Therefore, the workpiece is placed in a heating furnace, heated to 860℃±10 and kept warm for 3 hours, which can make the matrix of the workpiece completely austenitized and improve the tensile strength of the workpiece. The carbon potential in the furnace is 0.50, which is consistent with the camshaft material grade (50CrMoA grade has a carbon content of 0.5%) to prevent surface decarburization during the heating process.
[0044] After that, the workpiece is cooled in the cooling medium and then enters the cleaning machine to clean the oil stains; the cooling medium is Houghton HQG rapid quenching oil, and the cooling time is 30 minutes. During the cooling, it needs to be quickly stirred for 15 minutes to ensure uniform cooling;
[0045] After cooling, the workpiece enters the cleaning machine to clean the surface oil, and the cleaning time is 30 minutes.
[0046] Furthermore, the workpiece enters the tempering furnace for tempering, the tempering temperature is 650℃±10, preferably 650℃, and is kept warm before being taken out of the furnace and water-cooled; when the workpiece enters the tempering furnace for tempering, nitrogen is introduced into the tempering furnace to prevent the workpiece from oxidizing, and after keeping warm for 3 hours, it enters the cleaning machine for rapid cooling, which can avoid the second type of temper brittleness.
[0047] If tempering is carried out in the range of 400-650℃ and cooling is slow after tempering, the second type of temper brittleness will occur. When temper brittleness occurs, Ni, Cr, Sb, Sn, P, etc. will segregate to the original austenite grain boundaries and concentrate on the grain boundaries with a thickness of 2-3 atoms, reducing the strength of the parts. Temper brittleness increases with the increase of impurity elements.
[0048] 50CrMoA is high-quality 50CrMo steel, with less impurities such as S and P (sulfur and phosphorus), smaller fluctuation range of main components, and more stable quality. In this embodiment, 50CrMoA is selected as the camshaft base material for quenching and tempering, and high quenching temperature and high tempering temperature are selected. After tempering at 650°C, it enters the cleaning machine for rapid cooling, which can not only make the camshaft have better mechanical properties, but also avoid the occurrence of the second type of temper brittleness.
[0049] After the workpiece is tempered and fine-machined, it is subjected to medium-frequency quenching. First, the workpiece is placed on the quenching machine, and a profiling sensor is installed. The workpiece is subjected to multiple preheating cycle scanning heating to obtain a uniform hardened layer. After that, a spray ring is used for quenching and cooling. The final workpiece surface hardness is greater than 58HRC, and the hardened layer is 4.5-7mm.
[0050] If medium frequency quenching is performed directly after tempering, the presence of surface oxide scale will also affect the quenching effect and processing accuracy. In this embodiment, medium frequency quenching is performed after fine processing after tempering, and the surface is not affected by oxide scale. After medium frequency quenching, only fine grinding is required to complete the finished product processing, and the processing efficiency and accuracy are guaranteed.
[0051] During finishing, that is, the medium frequency stage, the operator operates the rotary arm to clamp the parts, and then selects the corresponding CNC machining program. The whole process runs automatically. After the medium frequency quenching is completed, the operator performs the unloading operation and then tempers it in time.
[0052] The EFD vertical induction hardening machine is used for medium frequency quenching. First, the profiling sensor is placed close to the base circle of the workpiece for preheating, so that the average temperature of the base circle is slightly higher than the temperature of the cam lobe tip. At this time, the preheating stops and waits for 5-10 seconds; then the profiling sensor returns to its initial position, performs cyclic scanning heating, and then quenches.
[0053] Specifically, for camshafts used in high-power diesel engines, the cams are relatively wide and the diameter difference between the cam base circle and the base body is only 7mm, and only 3.5mm on one side. When heated, the base circle will heat up slowly. However, by using multiple preheating cycle scanning heating methods, a uniform hardened layer can be obtained on large camshafts, and only fine grinding is required after medium frequency to complete the finished product processing, and the processing efficiency and accuracy are guaranteed.
[0054] The medium frequency profiling induction coil is not too uniform from the cam surface. The base circle diameter of the cam is 107mm, and the base circle diameter of the profiling sensor is 180mm. Since the diameter of the flanges at both ends is 177mm, it is impossible for the sensor to completely fit the cam surface contour, so it is still necessary to preheat at low power. After the prefabrication is completed, wait for 5-10 seconds to allow the heat to transfer and make the surface temperature more uniform. Then the profiling sensor returns to the initial position, and then high-power scanning heating and quenching are performed to meet the workpiece requirements.
[0055] EFD vertical induction hardening machine has three axes: Z, C, and Y. Z is up and down, C is rotation, and Y is front and back (the direction of the line connecting the cam lobe tip and the base circle). Install the profiling sensor on the machine. First, bring the profiling sensor close to the cam base circle (Y value minus 18mm), and then preheat. After preheating, the average temperature of the base circle is slightly higher than the temperature of the cam lobe tip. Wait for 5-10 seconds, increase the power, and then restore the sensor to the initial position (the center of the sensor and the center of the camshaft coincide), perform cyclic scanning heating, and then quench; the quenching cooling uses a spray ring. There are multiple spray holes evenly distributed on the spray ring.
[0056] The water flow pressure coming out of each water spray hole is consistent, which avoids the situation where the water flow pressure of the spray hole close to the water inlet is high and the water flow pressure of the spray hole far from the water inlet is low, which causes the cooling speed of various parts of the cam to be inconsistent during cooling, affecting the quenching effect. In this embodiment, the high-strength alloy camshaft rotates with the base during cooling to make the cooling process more uniform. The main spray flow rate is 90L / min and the auxiliary spray flow rate is 50L / min. It is tempered in a box-type tempering furnace at 170±10℃ for not less than 3h to eliminate stress and stabilize the structure. The dimensions of the camshaft before the intermediate frequency are shown in the figure. Figure 1-Figure 3 .
[0057] The medium frequency current frequency is 7000HZ, and the depth of the hardened layer can be changed by adjusting the heating time and power. The intake cam is on the top and the exhaust cam is on the bottom, and the distance between the two cams is small. When heating, the completed cam should be sprayed for protection to prevent annealing (the spray circle is divided into two parts, the upper part is the auxiliary spray area, and the lower part is the main spray area, which are connected to the corresponding pipes respectively). Among them, the cam base circle diameter is 107mm, the width is 35mm, the base diameter is 100mm, and the profile sensor base circle diameter is 180mm and the width is 20mm. The heating is divided into two stages, of which the preheating power of the first stage is 90KW, and the heating power of the second stage is 135Kw. The sensor moving speed is 260mm / min, and the moving distance is 15mm (the centerline position of the sensor corresponds to the centerline of the cam, and the upper and lower moving ranges are 7.5mm each). The sensor moving trajectory is as follows Figure 4-Figure 5 shown.
[0058] The camshaft has a base hardness of 28-32HRC after treatment, a surface hardness of more than 58HRC, a hardened layer of 4.5-7mm, and is evenly distributed. The quality of the high-power internal combustion engine camshaft produced by the above process is stable, and no quenching cracking has occurred in two years, and the service life is long. The processing process is relatively simple, which is conducive to large-scale production.
[0059] By optimizing the camshaft base material and performing the heat treatment method described in this embodiment, the camshaft of a high-power internal combustion engine meets the performance requirements. Moreover, no cracks have occurred in the nearly two years of production.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-strength alloy camshaft heat treatment process, characterized in that: The steps include: For quenching and tempering heat treatment, the workpiece is placed in a heating furnace, heated to 860℃±10 and kept warm, cooled in a cooling medium, and then sent to a cleaning machine to clean the oil stains; then sent to a tempering furnace for tempering, the tempering temperature is 650℃±10, and then taken out of the furnace for water cooling after keeping warm; After the workpiece is quenched and tempered and then finely machined, it is subjected to medium frequency quenching. The workpiece is placed on a quenching machine and a profile sensor is installed. The workpiece is subjected to multiple preheating cycle scanning heating to obtain a uniform hardened layer. After that, a spray ring is used for quenching cooling. The surface hardness of the workpiece is greater than 58HRC, and the hardened layer is 4.5-7mm. The heating furnace adopts the Aixilin multi-purpose furnace production line; The workpiece is placed in a heating furnace, heated to 860°C ± 10 and kept warm for 3 hours, the cooling medium is Houghton HQG rapid quenching oil, and cooled for 30 minutes; The camshaft material is 50CrMoA.
2. A high-strength alloy camshaft heat treatment process according to claim 1, characterized in that: When the workpiece enters the tempering furnace for tempering, nitrogen is introduced into the tempering furnace to prevent the workpiece from oxidation. After keeping warm for 3 hours, the workpiece enters the cleaning machine for rapid cooling.
3. A high-strength alloy camshaft heat treatment process according to claim 1, characterized in that: For medium frequency quenching, use EFD vertical induction quenching machine. First, place the profiling sensor close to the base circle of the workpiece for preheating, so that the average temperature of the base circle is slightly higher than the temperature of the cam lobe tip and wait for 5-10 seconds. The profile sensor then returns to its initial position, performs cyclic scanning heating, and then quenches.
4. A high-strength alloy camshaft heat treatment process according to claim 1, characterized in that: When the workpiece is cooled, the bottom cooperates with the base to rotate so that the cooling process is uniform.
5. A high-strength alloy camshaft heat treatment process according to claim 4, characterized in that: The spray circle includes an upper auxiliary spray area and a lower main spray area. The main spray flow rate is 90L / min and the auxiliary spray flow rate is 50L / min.
6. A high-strength alloy camshaft heat treatment process according to claim 3, characterized in that: The first-stage preheating power of the profiling sensor is 90KW, the second-stage cycle scanning heating power is 135Kw, and the sensor moving speed is 260mm / min.
7. The high-strength alloy camshaft heat treatment process according to claim 1, characterized in that: The frequency of the medium frequency current is 7000HZ.
8. The high-strength alloy camshaft heat treatment process according to claim 1, characterized in that: During medium frequency quenching, the intake cam is on top and the exhaust cam is on the bottom.
Citation Information
Patent Citations
Material for cam shaft and molding and manufacturing method of cam shaft
CN104278177A
Modified steel and its production method
CN1718826A
Double concave arc cam quenching process
CN1869255A