A beryllium-titanium alloy and its application in neutron breeder
By adjusting the composition and process of the beryllium-titanium alloy, a beryllium-titanium alloy with high temperature, high toughness and high neutron reproduction rate is formed, which solves the problems of radiation swelling and neutron reproduction performance degradation of beryllium materials in high-temperature environments, and achieves excellent radiation resistance. Swelling and mechanical properties, suitable for neutron reproduction and high temperature fields.
Patent Information
- Application Number
- CN202211648865.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-21
AI Technical Summary
Existing beryllium materials swell significantly due to radiation exposure in high-temperature commercial controlled fusion reactor environments, which affects reactor operation. Moreover, the addition of Ti in beryllium-titanium alloys results in reduced neutron breeding performance and poor toughness, making it difficult to meet high-temperature and high-toughness requirements.
Develop a beryllium-titanium alloy with a composition expression of Bea(TibMc)Xd, where M is a specific metal element and Proliferation rate and toughness, preparation methods include hot isostatic pressing, plasma sintering and powder metallurgy.
The beryllium-titanium alloy that achieves high temperature, high toughness and high neutron reproduction rate has excellent radiation swelling resistance and mechanical properties. It is suitable for the field of neutron reproduction and high-temperature materials, and provides a large composition range and wide preparation conditions.
Smart Images

Figure CN116024474B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a beryllium-titanium alloy and application thereof in a neutron breeder. Background Art
[0002] Nuclear fusion energy, as an internationally recognized clean energy, is gradually coming into people's view. In nuclear fusion reactors, the self-sustaining of tritium fuel is achieved through tritium breeder blankets. The tritium breeder blanket module designed with a ball bed of tritium breeder pellets and neutron breeder pellets alternately stacked is one of the blanket forms currently being studied. A large number of neutron breeder pellets in the blanket is conducive to improving the tritium breeding rate of the blanket and facilitating the diffusion and release of gas products such as helium and tritium.
[0003] Beryllium is an excellent neutron breeding material. The binding energy of beryllium neutrons in the nucleus is small (1.666MeV), which is equivalent to 1 / 5 to 1 / 6 of the energy of most stable atoms. Neutrons are released through the (n,2n) reaction, thereby achieving neutron proliferation. Metallic beryllium has no obvious irradiation swelling (<3%) below 400°C and transmutation He injection below 3000appm, and has been selected as the neutron breeder in the blanket of the ITER nuclear fusion reactor. However, the future commercial controlled fusion reactor (DEMO) will have a more harsh environment, higher operating temperature (600-900°C), greater irradiation dose, and helium injection of up to 20,000appm. The irradiation swelling of beryllium is particularly obvious (>3%), which may endanger the operation of the reactor.
[0004] Beryllium intermetallic compounds, such as Be 12 Ti has attracted the attention of researchers, and foreign countries, especially Japan, have paid attention to Be 12 Ti has been extensively studied. However, due to the addition of Ti, Be 12 The neutron multiplication performance of Ti is greatly reduced, and the toughness is very poor, which is extremely unfavorable for the production and use of beryllium titanium alloy and neutron breeder pellets. Therefore, the research of new beryllium titanium alloys with higher toughness and higher neutron multiplication performance is of great significance in the field of fusion neutron multiplication and even in the high temperature field. Summary of the invention
[0005] In order to overcome the above problems existing in the prior art, the present invention provides a beryllium-titanium alloy and its application in a neutron breeder, which are used to solve the above problems existing in the prior art.
[0006] A beryllium-titanium alloy, wherein the atomic percentage expression of the beryllium-titanium alloy material composition is Be a (Ti b M c )X d, where M is one or more of W, Re, Zr, Y, Mg, V, Mn, Fe, Co, Cr, Mo, Nb, Pb, Bi, Ta, Hf, Tl, X is one or more of O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, 75 ≤ a ≤ 97, 3 ≤ b ≤ 25, 0 ≤ c ≤ 25, 0 ≤ d ≤ 3, and a + b + c + d = 100.
[0007] For the aspects and any possible implementation manners described above, a further implementation manner is provided, wherein the grain size of the beryllium-titanium alloy ≤ 40 μm.
[0008] For the aspects and any possible implementation manners described above, a further implementation manner is provided, wherein when 0 < d ≤ 2, 0 ≤ c ≤ 3.84, c < b ≤ 7.69, 90.31 ≤ a ≤ 97, the beryllium-titanium alloy includes a tetragonal structure phase and a hexagonal close-packed structure phase, and the grain size ≤ 40 μm.
[0009] For the aspects and any possible implementation manners described above, a further implementation manner is provided, wherein when 0 < d ≤ 2, 0 ≤ c ≤ 5.26, 8.56 < b ≤ 10.53, 87.47 < a ≤ 92.31, the beryllium-titanium alloy includes a tetragonal structure phase and a trigonal structure phase, and the grain size ≤ 40 μm.
[0010] For the aspects and any possible implementation manners described above, a further implementation manner is provided, wherein when 0 < d ≤ 2, 0 ≤ c ≤ 5.26, c < b ≤ 8.56, 87.47 < a ≤ 92.31, the beryllium-titanium alloy includes a tetragonal structure phase and a hexagonal structure phase, and the grain size ≤ 40 μm.
[0011] For the aspects and any possible implementation manners described above, a further implementation manner is provided, wherein when 0 < d ≤ 2, 0 ≤ c ≤ 12.5, c < b ≤ 25, 73 ≤ a ≤ 89.47, the beryllium-titanium alloy includes a tetragonal structure phase and a trigonal structure phase, and the grain size ≤ 40 μm.
[0012] For the aspects and any possible implementation manners described above, a further implementation manner is provided, wherein the melting point of the beryllium-titanium alloy is greater than 1500 °C and the neutron multiplication factor is greater than 0.92.
[0013] For the aspects and any possible implementation manners described above, a further implementation manner is provided, wherein when d = 1.95, c = 2.37, b = 4.99, a = 90.69, the atomic percentage expression of the beryllium-titanium alloy material composition is Be 90.69 Ti 4.99 M 2.37 X 1.95 , which is composed of a tetragonal structure and a face-centered cubic structure phase, and the grain size ≤ 35 μm
[0014] According to the above aspects and any possible implementation, a further implementation is provided. When d=1.94, c=1.22, b=6.98, a=89.86, the atomic percentage expression of the composition of the beryllium titanium alloy material is Be 89.86 Ti 6.98 M 1.22 X 1.94 , including tetragonal structure and face-centered cubic structure phases, with grain size ≤35um.
[0015] The present invention also provides an application of a beryllium-titanium alloy with high temperature, high toughness and high neutron multiplication rate in a neutron multiplier.
[0016] Beneficial effects of the present invention
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The beryllium-titanium alloy with high temperature, high toughness and high neutron multiplication rate of the present invention has the atomic percentage expression of Be a (Ti b M c )X d , which has the following advantages:
[0019] 1. The beryllium-titanium alloy has a large composition range and a wide range of preparation conditions.
[0020] 2. By adjusting the alloy composition, heat treatment, hot and cold processing technology, etc., controlling the phase composition and refining the grains, different high-temperature properties, mechanical properties and neutron multiplication properties can be obtained.
[0021] 3. The main elements of the high-temperature, high-toughness, and high-neutron proliferation rate beryllium-titanium alloy material provided by the present invention are common metal raw materials and compounds, and can be prepared by different preparation methods, with the advantages of convenient preparation, simple process, and economy.
[0022] 4. The beryllium-titanium alloy prepared by the present invention has excellent high-temperature performance, a melting point exceeding 1500°C, a neutron multiplication rate exceeding 0.92, and excellent anti-irradiation swelling performance and mechanical properties.
[0023] 5. The beryllium-titanium alloy provided by the present invention has excellent mechanical properties, high temperature properties, excellent anti-irradiation swelling properties and neutron proliferation properties, and can be widely used in the fields of neutron proliferation, plasma-oriented materials and high temperature materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The microstructure diagram of the beryllium-titanium alloy of Example 1 of the present invention;
[0025] Figure 2 This is a microstructure diagram of the beryllium-titanium alloy of Example 3 of the present invention. DETAILED DESCRIPTION
[0026] In order to better understand the technical solution of the present invention, the content of the present invention includes but is not limited to the specific implementation methods described below, and similar technologies and methods should be considered to be within the scope of protection of the present invention. In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments.
[0027] It should be clear that the embodiments described in the present invention are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0029] The beryllium-titanium alloy with high toughness and high neutron multiplication rate of the present invention has the atomic percentage expression of Be a (Ti b M c )X d , where M is one or more of W, Re, Zr, Y, Mg, V, Mn, Fe, Co, Cr, Mo, Nb, Pb, Bi, Ta, Hf, Tl, X is one or more of O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, 75≤a≤97, 3≤b≤25, 0≤c≤25, 0≤d≤3, and a+b+c+d=100. If M is W, Be can be formed by controlling 95.65 W 4.35 The face-centered cubic phase has been tested to increase the neutron multiplication performance and toughness of the material; and other elements such as Zr and Y will also form corresponding "phases" under appropriate proportions and processes, thereby improving the overall performance of the entire alloy.
[0030] The beryllium titanium alloy of the present invention utilizes neutron breeding nuclides, large-sized atomic refractory metal elements and low-activation element doping, ductile phase assistance, and organizational control to obtain a beryllium titanium alloy with high toughness and high neutron breeding rate characteristics, and is applied to neutron breeding agents, plasma-facing and other structural and functional materials in high-temperature environments.
[0031] Furthermore, for the beryllium-titanium alloy with high toughness and high neutron multiplication rate of the present invention, its grain size ≤ 40um. As the grain size decreases, the strength and toughness of the alloy material will be improved.
[0032] Furthermore, when 0 < d ≤ 2, 0 ≤ c ≤ 3.84, c < b ≤ 7.69, 90.31 ≤ a ≤ 97, the beryllium-titanium alloy is composed of a tetragonal structure phase and a hexagonal close-packed structure phase, with a grain size ≤ 40um. The presence of the hexagonal close-packed beryllium phase will improve the neutron multiplication performance of the material and improve the toughness of the alloy. Combining grain size control further improves the material toughness.
[0033] Furthermore, when 0 < d ≤ 2, 0 ≤ c ≤ 5.26, 8.56 < b ≤ 10.53, 87.47 < a ≤ 92.31, the beryllium-titanium alloy is composed of a tetragonal structure and a trigonal structure phase, with a grain size ≤ 40um. Such as the tetragonal Be 92.31 Ti 7.69 phase and the trigonal α-Be 89.47 Ti 10.53 phase composition improves the tritium retention performance of the material. Combining grain size control further improves the material toughness.
[0034] Furthermore, when 0 < d ≤ 2, 0 ≤ c ≤ 5.26, c < b ≤ 8.56, 87.47 < a ≤ 92.31, the beryllium-titanium alloy is composed of a tetragonal structure and a hexagonal structure phase, with a grain size ≤ 40um. Such as the hexagonal β-Be 89.47 Ti 10.53 phase presence will improve the tritium retention performance, irradiation swelling resistance performance of the material and improve the toughness of the alloy. Combining grain size control further improves the material toughness.
[0035] Furthermore, when d = 1.94, c = 1.22, b = 6.98, a = 89.86, the atomic percentage expression of the beryllium-titanium alloy material composition is Be 89.86 Ti 6.98 M 1.22 X 1.94 , composed of a tetragonal structure and a face-centered cubic structure phase, with a grain size ≤ 35um. When M is Fe, the presence of the face-centered cubic Be 83.33 Fe 16.67 phase can significantly improve the toughness, processing performance and tritium retention performance of the material, and at the same time play a role in grain refinement, further improving the toughness of the material.
[0036] Furthermore, when 0 < d ≤ 2, 0 ≤ c ≤ 12.5, c < b ≤ 25, 73 ≤ a ≤ 89.47, the beryllium-titanium alloy is composed of a tetragonal structure and a trigonal structure phase, with a grain size ≤ 40um. Such as the trigonal Be 75 Ti 25The phase improves the tritium retention performance of the material, and combined with grain size control, further improves the toughness of the material.
[0037] Further, when d=1.95, c=2.37, b=4.99, a=90.69, the atomic percentage expression of the composition of the beryllium-titanium alloy material is Be 90.69 Ti 4.99 M 2.37 X 1.95 , composed of tetragonal structure and face-centered cubic structure phase, grain size ≤35um, face-centered cubic Be when M is Zr 92.86 Zr 7.14 The existence of the phase can significantly improve the neutron multiplication rate, high temperature performance, toughness, processing performance, tritium retention performance and radiation swelling resistance of the material, while also having the effect of grain refinement, further improving the toughness of the material.
[0038] The method for preparing the beryllium-titanium alloy of the present invention will now be described.
[0039] The method for preparing beryllium-titanium alloy and neutron-breeding beryllium-titanium spheres by using the alloy comprises hot isostatic pressing, plasma sintering, rotating electrode method and powder metallurgy method.
[0040] The preparation of beryllium titanium alloy by hot isostatic pressing includes the following steps:
[0041] S1. Mix pure beryllium powder, titanium powder and other raw materials according to the chemical composition ratio;
[0042] S2. Then the metal powders are mixed and filled into the cladding for high vacuum sealing and pressed into ingots by hot isostatic pressing. The manufacturing conditions at this time are as follows:
[0043] Pressure: 100~1000MPa,
[0044] Temperature: 700~1300℃,
[0045] Time: 0.5~6h.
[0046] The plasma sintering method for preparing beryllium titanium alloy includes the following steps:
[0047] S1. Mix pure beryllium powder, titanium powder and other raw materials according to the chemical composition ratio;
[0048] S2. Then mix the metal powders in the right proportions, and then perform vacuum plasma rapid sintering to form the product. The sintering conditions at this time are described as follows:
[0049] Vacuum degree: 1×10 -1 Pa~1×10 -10 Pa temperature: 700~1300℃
[0050] Time: 0.5~6h
[0051] Powder Metallurgy:
[0052] The method is used to manufacture neutron breeding beryllium titanium microspheres. First, the beryllium titanium alloy obtained by the above preparation method is used as the material for manufacturing neutron breeding. Then the material is loaded into a mold, crushed, and spheroidized to obtain the neutron breeding beryllium titanium microspheres.
[0053] Rotating electrode method:
[0054] In order to prepare the neutron breeding agent beryllium titanium alloy microspheres of the present invention by the rotating electrode method, it is necessary to first prepare the consumable electrode beryllium titanium alloy rods. The beryllium titanium alloy prepared by the aforementioned hot isostatic pressing method, plasma sintering method or smelting method is used as the consumable electrode material, and the material is machined to produce a specified electrode shape. Next, the prepared consumable electrode is used to manufacture the neutron breeding beryllium titanium microspheres by the rotating electrode method. The manufacturing conditions at this time are not particularly limited, and the description of the preferred conditions is as follows:
[0055] Atmosphere gas pressure: 60MPa~1100MPa
[0056] Arc current: 100~1000A
[0057] Consumable electrode rotation speed: 5~1000m / s.
[0058] [Example]
[0059] Example 1
[0060] A beryllium-titanium alloy with high toughness and high neutron proliferation rate, the composition of which is: Be: 89.86at.%, Ti: 6.98at.%, Fe: 1.22at.%, O: 0.08at.%, other elements include C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, the total content is about 1.86at.%, the atomic percentage expression of the alloy material composition is Be 89.86 Ti 6.98 Fe 1.22 X 1.94 The hot isostatic pressing method was used to prepare the material at a temperature of 1000°C and a time of 1.5 h. The microstructure of the material is shown in Figure 1 As shown, the alloy can be composed of tetragonal Be 92.31 Ti 7.69 and face-centered cubic Be 83.33 Fe 16.67 Phase composition, grain size ≤15um, neutron multiplication performance of about 0.92, high temperature performance and anti-irradiation swelling performance are excellent, the properties are shown in Table 1, indicating that the alloy can be used in the field of neutron multiplication, plasma-oriented materials and high temperature fields.
[0061] Table 1
[0062]
[0063] The properties in Table 1 are described as follows.
[0064] Neutron multiplication performance refers to the neutron multiplication performance of the elements that constitute the alloy, and is evaluated by the neutron multiplication rate. Considering that beryllium is a naturally excellent neutron multiplication material, beryllium is used as a comparison material (the neutron multiplication rate is set to 1). The closer the performance of other materials is to 1, the better the neutron multiplication performance.
[0065] Tritium retention performance (tritium can be injected externally and then tested for its retention in the material, which is a test of material performance). Since the purpose of fusion neutron breeder is to achieve self-sustaining tritium fuel, the retention of tritium in the material is also very important. A temperature decomposition gas analyzer (TDS) is used to measure tritium retention. That is, according to the degree of tritium retention, it can be excellent (very little retention), medium (partial retention), or poor (a lot of retention).
[0066] Anti-radiation swelling performance. Neutron irradiation materials will produce a large number of vacancies. These vacancies will further migrate and aggregate to form vacancy clusters such as holes, causing the volume swelling of the material. Under the conditions of high temperature 400℃ and helium injection of 3000appm, the irradiation swelling rate of metallic beryllium is >3%, endangering the safe operation of the reactor. It is assumed to have poor anti-swelling performance, and it is used as a comparison. The irradiation swelling rate is 1-3%, which is medium, and the irradiation swelling rate is less than 1%, which is excellent.
[0067] Other properties are well known in the industry and will not be specifically described. Due to differences in material composition, heat treatment process, hot and cold processing process, etc., the phase composition, grain size, etc. of the material are different, thereby regulating the various properties of the material. For example, when M is Fe, the appropriate component ratio and process can make the grain size of the material less than 15um, and the formation of a tough high-temperature phase greatly improves the toughness, processing performance and tritium retention performance of the material. For example, when M is Zr, the appropriate component ratio and process can refine the grains of the material to form a beryllium zirconium auxiliary phase that is resistant to high temperature and has a high neutron proliferation rate and high toughness, greatly improving the material's neutron proliferation rate, high temperature performance, toughness, processing performance, tritium retention performance and anti-radiation swelling performance.
[0068] Example 2
[0069] A beryllium-titanium alloy with high toughness and high neutron proliferation rate, comprising: Be: 90.32at.%, Ti 7.76at.%, and other elements including O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, and U with a total content of about 1.92at.%, prepared by plasma sintering at a temperature of 1000°C for 1.5 hours and vacuum annealing at 1200°C for 2 hours. The beryllium-titanium alloy is composed of a tetragonal structure of Be 92.31 Ti 7.69 and hexagonal β-Be 89.47 Ti 10.53 Phase composition, grain size ≤40um, neutron multiplication rate greater than 0.90, excellent radiation swelling resistance, and the properties are shown in Table 1 above, indicating that the alloy can be used in the field of neutron multiplication, plasma-facing materials and high-temperature fields.
[0070] Example 3
[0071] A beryllium-titanium alloy with high toughness and high neutron proliferation rate, the composition of which is: Be: 90.69at.%, Ti: 4.99at.%, Zr: 2.37at.%, O: 0.08at.%, other elements include C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U with a total content of about 1.87at.%, the atomic percentage expression of the alloy material composition is Be 90.69 Ti 4.99 Zr 2.37 X 1.95 , prepared by plasma sintering method, temperature 1000 ℃, time 1.5h, the material microstructure is as follows Figure 2 As shown, the alloy can be composed of tetragonal Be 92.31 Ti 7.69 and face-centered cubic structure Be 92.86 Zr 7.14 Phase composition, average grain size ≤ 25um, neutron multiplication performance exceeds 0.92, high temperature performance and radiation swelling resistance are excellent, and the properties are shown in Table 1, indicating that the alloy can be used in the field of neutron multiplication, plasma-oriented materials and high temperature fields.
[0072] Example 4
[0073] A beryllium-titanium alloy with high toughness and high neutron proliferation rate, the composition of which is: Be: 90.48at.%, (Ti+M): 7.54at.%, and the content of Ti is greater than M, wherein M is one or more of W, Re, Y, V, Mn, Fe, Co, Cr, Mo, Nb, Pb, Bi, Ta, Hf, Tl, and other elements include O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, and U. The total content is about 1.98at.%, and the atomic percentage expression of the alloy material composition is Be 90.69 (Ti, M) 7.54 X 1.98 , prepared by hot isostatic pressing at 1000℃ for 2.0h. The alloy consists of Be 92.31 Ti 7.69 and Be 92.31 M 7.69 Phase composition, average grain size ≤40um, neutron multiplication performance of about 0.92, excellent toughness and resistance to radiation swelling, the properties are shown in Table 1, indicating that the alloy can be used in the field of neutron multiplication, plasma-oriented materials and high temperature fields.
[0074] The above description shows and describes several preferred embodiments of the present invention, but as mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not depart from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
Claims
1. A beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron multiplication rate, characterized in that: The atomic percentage expression of the beryllium-titanium alloy material composition is Be a Ti b M c X d , where M is Fe, X is one or more of O, C, N, P, S, Si, Al, Ca, Sc, Ni, Cu, U, 75 ≤ a ≤ 97, 3 ≤ b ≤ 25, 0 < c ≤ 25, 0 ≤ d ≤ 3, and a + b + c + d = 100.
2. The beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron multiplication rate according to claim 1, characterized in that: The grain size of the beryllium-titanium alloy is ≤ 40 μm.
3. The beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron multiplication rate according to claim 1, characterized in that: When 0 < d ≤ 2, 0 < c ≤ 3.84, c < b ≤ 7.69, 90.31 ≤ a ≤ 97, the beryllium-titanium alloy includes a tetragonal structure phase and a hexagonal close-packed structure phase, and the grain size is ≤ 40 μm.
4. The beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron multiplication rate according to claim 1, characterized in that: When 0 < d ≤ 2, 0 < c ≤ 5.26, 8.56 < b ≤ 10.53, 87.47 < a ≤ 92.31, the beryllium-titanium alloy includes a tetragonal structure phase and a trigonal structure phase, and the grain size is ≤ 40 μm.
5. The beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron multiplication rate according to claim 1, characterized in that: When 0 < d ≤ 2, 0 < c ≤ 5.26, c < b ≤ 8.56, 87.47 < a ≤ 92.31, the beryllium-titanium alloy includes a tetragonal structure phase and a hexagonal structure phase, and the grain size is ≤ 40 μm.
6. The beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron multiplication rate according to claim 1, characterized in that: When 0 < d ≤ 2, 0 < c ≤ 12.5, c < b ≤ 25, 73 ≤ a ≤ 89.47, the beryllium-titanium alloy includes a tetragonal structure phase and a trigonal structure phase, and the grain size is ≤ 40 μm.
7. The beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron multiplication rate according to claim 1, characterized in that: When d=1.94, c=1.22, b=6.98, a=89.86, the atomic percentage expression of the composition of the beryllium-titanium alloy material is Be 89.86 Ti 6.98 M 1.22 X 1.94 , including tetragonal structure and face-centered cubic structure phases, with grain size ≤35um.
8. The beryllium-titanium multi-element alloy with high temperature, high toughness and high neutron proliferation rate according to claim 1, characterized in that: When d=1.95, c=2.37, b=4.99, a=90.69, the atomic percentage expression of the composition of the beryllium-titanium alloy material is Be 90.69 Ti 4.99 M 2.37 X 1.95 , including tetragonal structure and face-centered cubic structure phases, with grain size ≤35um.
9. Use of the beryllium-titanium multi-element alloy according to any one of claims 1 to 8 in a neutron breeder.
Citation Information
Patent Citations
Method for preparing beryllium-titanium alloy by carrying out spark plasma sintering
CN104630524A
Material including beryllium intermetallic compound and having excellent high-temperature property applied to nuclear fusion reactor
US20050135960A1
Material for nuclear fusion furnace excellent in high temperature characteristics comprising beryllium intermetallic compound
WO2003085678A1