A production method for reducing edge fraying during cold rolling of nickel-saving austenitic stainless steel
By adjusting the alloy composition and heating process parameters of nickel-free austenitic stainless steel, the problem of edge scaling defects during cold rolling is solved, the scaling defect rate is reduced, and product quality is improved.
Patent Information
- Application Number
- CN202211694428.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-28
AI Technical Summary
Nickel-free austenitic stainless steel is prone to edge scaling defects during the cold rolling process. Existing solutions cannot effectively solve it, affecting its subsequent production and application.
By adjusting the alloy composition and heating process parameters, control the contents of C, Cr, Mn, and N, set the tensioning and straightening temperature at 920-960°C, and reduce the temperature difference through temperature control of the heat recovery section and the preheating section during the heating process. Stress, reducing grain boundary weakening and columnar crystal cracking.
It effectively reduces the edge scale defect rate under the cold assembly method from 22.66% to less than 2.02%, improving product quality and market competitiveness.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of smelting, continuous casting and heating production, and particularly relates to a production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel. Background Art
[0002] Nickel-saving austenitic stainless steel is an economical stainless steel that reduces the use of precious metals and replaces nickel with elements such as manganese and nitrogen on the basis of traditional austenitic stainless steel. It has developed rapidly in China in recent years. Its good machining performance, good corrosion resistance and glossy surface have become hard conditions for its market promotion.
[0003] Nickel-saving austenitic stainless steel is a new type of cheap stainless steel developed in China in recent years, mainly used in civilian products. Its standard composition range (wt.%) is: C: 0.10% ~ 0.15%, Mn: 9% ~ 12%, Si: 0.3% ~ 0.7%, P: ≤ 0.060%, S: ≤ 0.030%, Cr: 13% ~ 14.5%, Ni: 0 ~ 2%, N: 0.17% ~ 0.2%, Cu: 0 ~ 0.5%, the rest is iron and trace elements and impurities. However, although the use of manganese, nitrogen and other elements to replace nickel reduces the cost of austenitic stainless steel, at the same time, it also reduces the stability of stainless steel austenite, and it is easy to have scale defects within 100mm from the edge during the subsequent hot rolling process, which has a negative impact on the mechanical properties and corrosion resistance of the plate, affecting the economic benefits.
[0004] During the heating process of the cold-charging furnace casting, a large amount of precipitation occurs at the grain boundaries of the solidification structure, the degree of grain boundary weakening is greater than that of the hot-charging furnace casting, and the temperature difference between the surface and the core in the initial stage of heating is higher than that of the hot-charging furnace casting, which will cause greater stress concentration at the edge of the casting, resulting in the sensitivity of the scale defect to the cold-charging furnace method is much greater than that of the hot-charging furnace method, and the scale defects that occur in the hot rolling stage cannot be repaired in subsequent processing. At present, the main solution to the linear and peeling defects caused by scale defects is to grind the surface of the slab or to remove the scale using hot rolling descaling equipment. However, when the metastable nickel-saving austenitic stainless steel is cold-charged, the problem of more scale defects within 100mm of the edge of the steel coil cannot be solved well by the above methods. The above problems affect the subsequent production and application of nickel-saving austenitic stainless steel, so it is necessary to design a more suitable processing technology for the cold-charging furnace method of nickel-saving austenitic stainless steel. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a production method for reducing edge fraying during cold rolling of nickel-saving austenitic stainless steel.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] A production method for reducing edge folding of nickel-saving austenitic stainless steel during cold rolling, comprising the following steps:
[0008] (1) Smelting: According to the mass percentage, the C, Cr, Mn and N contents of nickel-saving austenitic stainless steel are controlled, C: 0.11%-0.119%; Cr: 13.65%-14.05%; Mn: 9.29%-9.69%; N: 0.157%-0.177%;
[0009] (2) Continuous casting:
[0010] (3) Heating: After the continuous casting ingot is cast, cut into slabs, it is sent to a heating furnace for heating. The total heating time in the furnace is controlled at 260-265 minutes.
[0011] Furthermore, in step (1), except for C, Cr, Mn and N, the contents of other components of the nickel-saving austenitic stainless steel are controlled within the standard range.
[0012] Furthermore, the casting superheat in step (1) is selected to be a minimum value of 25° C. within the allowable range.
[0013] Furthermore, the straightening temperature of the continuous casting in step (2) is 920-960°C.
[0014] Furthermore, in step (3), the temperature of the slab sent into the heating furnace by cold charging is 25°C.
[0015] Furthermore, in step (3), the heating process of the heating furnace is heated through a heat recovery section, a preheating section, a first heating section, a second heating section, and a soaking section.
[0016] Furthermore, in step (3), the temperature of the heat recovery section is 654-714°C, the heating time is 100-109 minutes, the temperature of the preheating section is 853-913°C, the heating time is 30-35 minutes, the temperature of the first heating section is 1119-1247°C, the temperature of the second heating section is 1247-1270°C, the temperature of the equalizing section is 1266-1270°C, and the total time for the first and second heating sections is 80-85 minutes.
[0017] Furthermore, the applicable specifications of the slab cut after casting in step (3) are: 11500×200×1000mm.
[0018] The principle of the present invention is:
[0019] Through electron scanning microscope microscopic analysis of a large number of steel coils with scale defects within 100mm of the edge, it was found that there was no protective slag and inclusions at the defect location, the matrix structure near the defect was normal and not affected by overheating defects. In practice, it was found that the generation of scale defects in this type of steel had no direct connection with the original defects on the surface of the ingot. The slabs produced by conventional processes were selected and the surface was evenly polished. After eliminating the influence of defects such as cracks on the surface, conventional processes were used for heating and rolling. After pickling, it was found that the scale defects in the corresponding area of the edge did not decrease.
[0020] Further analysis of the ingot revealed that the columnar crystals of the nickel-free austenitic stainless steel were too developed, and there was almost no chilled fine-grained layer structure on the surface. In addition, there were a large number of chromium carbide precipitation phases at the grain boundaries of the solidified structure, and there was an obvious grain boundary weakening phenomenon. As for the structure close to the surface, there was oxidation at the grain boundaries. As for the columnar crystal structure, the columnar crystal structure almost ran through the entire thickness direction, and the grain boundaries between the columnar crystals were coarse. There were a large number of precipitations between the crystals, resulting in poor bonding between each other. During the heating and hot rolling process, the columnar crystals were very easy to crack and cause linear and detached scales and mountain scales.
[0021] Based on the above research on the scale-break defects of the hot-rolled curling edge of nickel-saving austenitic stainless steel, in order to solve the problem of high defect rate of cold charging method for this type of steel, the present invention partially adjusts the production process parameters of the cold charging method, firstly adjusts the alloy element composition (wt.%) of this type of steel, keeps C at 0.11%-0.119%, Cr at 13.65%-14.05%, Mn at 9.29%-9.69%, N at 0.157%-0.177%, and the casting superheat is 25°C; in terms of composition control, the peritectic point is moved to the right, so that this type of steel is away from the violent peritectic reaction during the cooling and solidification process, and the surface depression, grain boundary cracks and overdeveloped columnar crystals caused by this reaction are avoided to a certain extent, and the intercrystalline bonding force is improved from the source, and with a certain superheat, casting speed and appropriate cooling intensity, the columnar crystal size of the ingot is relatively uniform, which improves The surface quality of the original ingot is improved, and a better original solidification structure of the ingot is obtained; by setting the straightening temperature at 920-960℃, the brittle temperature range of 750-900℃ of nickel-saving austenitic stainless steel is avoided; then, in order to prevent the ingot from being heated in the heating furnace by cold loading, the temperature gradient inside and outside the ingot is large, and a stress concentration area is generated at the edge of the ingot, which destroys the columnar crystals and causes micro cracks, so the heat recovery section and preheating section where temperature difference stress concentration occurs are adjusted, wherein the heat recovery section temperature is 654-714℃, the heating time is 100-109 minutes, the preheating section temperature is 853-913℃, and the heating time is 30 minutes, so that the heating process in the heating furnace is slowly heated. Through the control of heat recovery and preheating section temperature, the problem of excessive temperature gradient in the initial heating stage caused by the large temperature difference between the ingot and the heating furnace under the condition of cold loading at 25℃ can be alleviated, and the expansion of micro cracks at the edge caused by increased stress between columnar crystals can be slowed down. In addition, the heating system can also make a large number of precipitated phases existing in the grain boundaries of the cold-charged ingot solidification structure be integrated into the matrix as much as possible, reducing the degree of grain boundary weakening. The various steps in the process of the present invention are closely linked and indispensable, and ultimately reduce the edge scale defects of nickel-saving austenitic stainless steel during cold charging from 22.66% to within 2.02%, effectively controlling the defect rate and improving product quality and market competitiveness.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) The present invention optimizes the alloy composition of nickel-saving austenitic stainless steel from the perspective of the influence of different alloy compositions on phase transformation parameters, reduces the sensitivity of scale defects to cold charging furnace mode and subsequent processing, and achieves a good optimization effect.
[0024] 2) The present invention designs a billet straightening temperature zone based on the brittle temperature range angle of nickel-saving austenitic stainless steel, which has a good effect on reducing the sensitivity of scale fracture defects.
[0025] 3) The present invention accelerates the integration of the precipitated phase into the matrix, reduces the degree of grain boundary weakening and reduces the angle of the temperature difference stress at the edge in the initial stage of cold charging. Under the condition of cold charging, i.e., sending the product into the heating furnace at 25°C, the present invention proposes a heating system that reduces the sensitivity of scale defects by adjusting the heating temperature and time interval of the heat recovery section and reducing the heating rate of the preheating section, which provides a direction for optimizing the heating system of the cold charging method. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0027] Embodiment 1:
[0028] A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel, comprising the following steps:
[0029] 1) Smelting: Smelting composition (wt.%): C content is 0.11%, Cr content is 13.65%, Mn content is 9.29%, N content is 0.157%, Ni content is 1.24%, Si content is 0.41%, Cu content is 0.31%, B content is 0.0009%, and the rest is iron and microscopic impurities. The casting superheat is 25℃;
[0030] 2) Continuous casting: The straightening temperature of the ingot is 960°C;
[0031] 3) Heating: After the ingot is cast and cut into slabs (specifications 11500×200×1000mm), it is immediately sent to the hot rolling heating furnace for heating, and the temperature of the slab sent to the heating furnace is 25°C; the heating process in the heating furnace slowly heats up through the heat recovery section, preheating section, heating section one, heating section two, and soaking section, wherein the temperature of the heat recovery section is 654°C, the heating time is 100 minutes, the temperature of the preheating section is 853°C, and the heating time is 30 minutes; the temperature of the heating section one is 1119°C, the temperature of the heating section two is 1247°C, the temperature of the soaking section is 1266°C, the total time for the heating sections one and two is 80 minutes, and the soaking section time is 50 minutes.
[0032] Embodiment 2:
[0033] A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel, comprising the following steps:
[0034] 1) Smelting: Smelting composition (wt.%): C content is 0.119%, Cr content is 14.05%, Mn content is 9.69%, N content is 0.177%, Ni content is 1.24%, Si content is 0.41%, Cu content is 0.31%, B content is 0.0009%, and the rest is iron and microscopic impurities. The casting superheat is 25℃;
[0035] 2) Continuous casting: The straightening temperature of the ingot is 960°C;
[0036] 3) Heating: After the ingot is cast and cut into slabs (specifications 11500×200×1000mm), it is immediately sent to the hot rolling heating furnace for heating, and the temperature of the slab sent to the heating furnace is 25°C; the heating process in the heating furnace slowly increases the temperature through the heat recovery section, preheating section, heating section one, heating section two, and soaking section, wherein the temperature of the heat recovery section is 684°C, the heating time is 100 minutes, the temperature of the preheating section is 883°C, and the heating time is 30 minutes; the temperature of the heating section one is 1119°C, the temperature of the heating section two is 1247°C, the temperature of the soaking section is 1266°C, the total time for the heating sections one and two is 85 minutes, and the soaking section time is 50 minutes.
[0037] Embodiment 3:
[0038] A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel, comprising the following steps:
[0039] 1) Smelting: Smelting composition (wt.%): C content is 0.115%, Cr content is 13.85%, Mn content is 9.49%, N content is 0.157%, Ni content is 1.24%, Si content is 0.41%, Cu content is 0.31%, B content is 0.0009%, and the rest is iron and microscopic impurities. The casting superheat is 25℃;
[0040] 2) Continuous casting: The straightening temperature of the ingot is 960°C;
[0041] 3) Heating: After the ingot is cast and cut into slabs (specifications 11500×200×1000mm), it is immediately sent to the hot rolling heating furnace for heating, and the temperature of the slab sent to the heating furnace is 25°C; the heating process in the heating furnace slowly heats up through the heat recovery section, preheating section, heating section one, heating section two, and soaking section, wherein the temperature of the heat recovery section is 714°C, the heating time is 100 minutes, the temperature of the preheating section is 913°C, and the heating time is 30 minutes; the temperature of the heating section one is 1150°C, the temperature of the heating section two is 1250°C, the temperature of the soaking section is 1266°C, the total time for the heating sections one and two is 80 minutes, and the soaking section time is 50 minutes.
[0042] Embodiment 4:
[0043] A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel, comprising the following steps:
[0044] 1) Smelting: Smelting composition (wt.%): C content is 0.11%, Cr content is 14.05%, Mn content is 9.29%, N content is 0.177%, Ni content is 1.24%, Si content is 0.41%, Cu content is 0.31%, B content is 0.0009%, and the rest is iron and microscopic impurities. The casting superheat is 25℃;
[0045] 2) Continuous casting: The straightening temperature of the ingot is 920°C;
[0046] 3) Heating: After the ingot is cast and cut into slabs, it is immediately sent to the hot rolling heating furnace for heating. The temperature of the slab sent to the heating furnace is 25°C; the heating process in the heating furnace slowly increases the temperature through the heat recovery section, preheating section, heating section one, heating section two, and soaking section, wherein the temperature of the heat recovery section is 714°C, the heating time is 100 minutes, the temperature of the preheating section is 913°C, and the heating time is 30 minutes; the temperature of the heating section one is 1150°C, the temperature of the heating section two is 1250°C, the temperature of the soaking section is 1266°C, the total time of the heating sections one and two is 85 minutes, and the soaking section time is 50 minutes.
[0047] Embodiment 5:
[0048] A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel, comprising the following steps:
[0049] 1) Smelting: Smelting composition (wt.%): C content is 0.119%, Cr content is 14.05%, Mn content is 9.29%, N content is 0.177%, Ni content is 1.24%, Si content is 0.41%, Cu content is 0.31%, B content is 0.0009%, and the rest is iron and microscopic impurities. The casting superheat is 25℃;
[0050] 2) Continuous casting: The straightening temperature of the ingot is 930°C;
[0051] 3) Heating: After the ingot is cast and cut into slabs, it is immediately sent to the hot rolling heating furnace for heating. The temperature of the slab sent to the heating furnace is 25°C; the heating process in the heating furnace slowly increases the temperature through the heat recovery section, preheating section, heating section one, heating section two, and soaking section, wherein the temperature of the heat recovery section is 714°C, the heating time is 100 minutes, the temperature of the preheating section is 913°C, and the heating time is 30 minutes; the temperature of the heating section one is 1119°C, the temperature of the heating section two is 1260°C, the temperature of the soaking section is 1266°C, the total time of the heating sections one and two is 80 minutes, and the soaking section time is 55 minutes.
[0052] Embodiment 6:
[0053] A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel, comprising the following steps:
[0054] 1) Smelting: Smelting composition (wt.%): C content is 0.11%, Cr content is 14.05%, Mn content is 9.29%, N content is 0.177%, Ni content is 1.24%, Si content is 0.41%, Cu content is 0.31%, B content is 0.0009%, and the rest is iron and microscopic impurities. The casting superheat is 25℃;
[0055] 2) Continuous casting: The straightening temperature of the ingot is 940°C;
[0056] 3) Heating: After the ingot is cast and cut into slabs, it is immediately sent to the hot rolling heating furnace for heating. The temperature of the slab sent to the heating furnace is 25°C; the heating process in the heating furnace slowly increases the temperature through the heat recovery section, preheating section, heating stage 1, heating stage 2, and soaking section, wherein the temperature of the heat recovery section is 714°C, the heating time is 100 minutes, the temperature of the preheating section is 913°C, and the heating time is 30 minutes; the temperature of the heating stage 1 is 1119°C, the temperature of the heating stage 2 is 1247°C, the temperature of the soaking section is 1270°C, the total time for the heating stages 1 and 2 is 85 minutes, and the soaking section time is 50 minutes.
[0057] Embodiment 7:
[0058] A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel, comprising the following steps:
[0059] 1) Smelting: Smelting composition (wt.%): C content is 0.11%, Cr content is 14.05%, Mn content is 9.29%, N content is 0.177%, Ni content is 1.24%, Si content is 0.41%, Cu content is 0.31%, B content is 0.0009%, and the rest is iron and microscopic impurities. The casting superheat is 25℃;
[0060] 2) Continuous casting: The straightening temperature of the ingot is 950°C;
[0061] 3) Heating: After the ingot is cast and cut into slabs, it is immediately sent to the hot rolling heating furnace for heating. The temperature of the slab sent to the heating furnace is 25°C; the heating process in the heating furnace slowly increases the temperature through the heat recovery section, preheating section, heating stage 1, heating stage 2, and soaking section, wherein the temperature of the heat recovery section is 714°C, the heating time is 100 minutes, the temperature of the preheating section is 913°C, and the heating time is 30 minutes; the temperature of the heating stage 1 is 1150°C, the temperature of the heating stage 2 is 1260°C, the temperature of the soaking section is 1270°C, the total time for the heating stages 1 and 2 is 80 minutes, and the soaking section time is 50 minutes.
[0062] The remaining processes in the above embodiment are conventional processes. In the above embodiment, a total of 4406 rolls of nickel-reduced austenitic stainless steel strips were rolled. After pickling, the quality inspector visually observed that 89 rolls were downgraded with edge scale defects, and the defect rate was 2.02%. From the actual situation of mass production, the defect rate was effectively controlled.
[0063] The present invention maintains C at 0.11%-0.119%, Cr at 13.65%-14.05%, Mn at 9.29%-9.69%, N at 0.157%-0.177%, and the casting superheat is 25°C, all of which are to avoid violent peritectic reaction during the cooling and molding process of the ingot, thereby forming a good solidification structure, reducing grain boundary cracks and surface depressions, and reducing the degree of development of columnar crystals, and to obtain a better quality raw material by cold charging as much as possible. The billet is cast at the beginning; the billet straightening temperature is set at 920-960℃, avoiding the brittle temperature range of 750-900℃ for nickel-saving austenitic stainless steel; during the heating process, considering that the billet is kept at 25℃ in the cold charging mode and the temperature in the heating furnace is too large, resulting in stress concentration in the heat recovery section and preheating section at the initial heating stage, the heat recovery section temperature is set to 654-714℃, the heating time is 100 minutes, and the preheating section temperature is set to 853-913℃, and the heating time is 30 minutes. The temperature gradient inside and outside the billet is controlled at about 280℃, the temperature gradient between the center and the edge of the slab is reduced, the temperature difference stress is reduced, cracking is avoided, and the influence of the temperature difference stress and grain boundary weakening on the billet quality is minimized in combination with reducing the grain boundary weakening angle caused by the precipitation phase at the grain boundary. The present invention aims at the surface quality and solidification structure of nickel-saving austenitic stainless steel, and proposes the problem that due to the large thermal stress in the initial stage of heating in a cold-charging furnace, more scale-fracture defects are generated after hot rolling than those generated after hot charging. The invention proposes reducing the severity of the peritectic reaction, improving the original solidification structure of the ingot, reducing the large temperature difference stress in the initial stage of heating, etc., thereby providing a control process and improvement direction for reducing the generation rate of scale-fracture defects.
[0064] The above technical scheme explains the technical idea of the present invention, which cannot be used to limit the protection scope of the present invention. Any changes and modifications made to the above technical scheme based on the technical essence of the present invention without departing from the content of the technical scheme of the present invention shall fall within the protection scope of the technical scheme of the present invention.
Claims
1. A production method for reducing edge folding during cold rolling of nickel-saving austenitic stainless steel, characterized in that: The steps include: (1) Smelting: According to the mass percentage, the C, Cr, Mn and N contents of nickel-saving austenitic stainless steel are controlled, C: 0.11%-0.119%; Cr: 13.65%-14.05%; Mn: 9.29%-9.69%; N: 0.157%-0.177%; (2) Continuous casting; (3) Heating: After the continuous casting ingot is cast and cut into slabs, it is sent to the heating furnace for heating. The total heating time in the furnace is controlled at 260-265 minutes; Among them, the temperature of the slab sent into the heating furnace by cold loading in step (3) is 25°C.
2. A method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel according to claim 1, characterized in that: In step (1), the casting superheat is set to a minimum value of 25°C within the allowable range.
3. The method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel according to claim 1, characterized in that: The straightening temperature of the continuous casting billet in step (2) is 920-960°C.
4. The method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel according to claim 1, characterized in that: In step (3), the heating process of the heating furnace is heated through a heat recovery section, a preheating section, a first heating section, a second heating section, and a soaking section.
5. A production method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel according to claim 4, characterized in that: The temperature of the heat recovery section is 654-714°C, the heating time is 100-109 minutes, the temperature of the preheating section is 853-913°C, the heating time is 30-35 minutes, the temperature of the first heating section is 1119-1247°C, the temperature of the second heating section is 1247-1270°C, the temperature of the equalizing section is 1266-1270°C, and the total time for heating the first and second sections is 80-85 minutes.
6. The method for reducing edge folding of cold-rolled nickel-saving austenitic stainless steel according to claim 1, characterized in that: The applicable specifications of the slab cut after casting in step (3) are: 11500×200×1000mm.