Stainless steel strip and method for manufacturing the same
Through four-step heat treatment process, including solid solution, adjustment, cold treatment and aging treatment, the fatigue strength and mechanical properties of the 14-7PH stainless steel belt are improved, and the deformation and fatigue crack problems during operation in the press are solved, achieving the performance of HT1770M index.
Patent Information
- Application Number
- CN202211658532.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-22
AI Technical Summary
When the existing 14-7PH stainless steel belts are run in the press, it is difficult to have high fatigue strength and mechanical properties at the same time, and deformation and fatigue cracks caused by roller wear are prone to occur.
Four-step heat treatment processes are adopted: solid solution treatment, adjustment treatment, cold treatment and aging treatment, including heating to solid solution temperature, adjusting temperature, cooling to room temperature, and insulated at low temperatures, and finally aging treatment. The specific steps and temperature parameters are adjusted to Improve the fatigue strength and mechanical properties of steel belts.
Through this process, the fatigue strength of the steel belt reaches more than 90% of HT1770M, the yield strength and tensile strength are significantly improved, and the Rockwell hardness is also improved, solving the problems of deformation and fatigue cracks.
Smart Images

Figure CN116024496B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a stainless steel strip and a manufacturing method thereof. Background Art
[0002] Stainless steel precision transmission belt is used in continuous hot presses for fiberboard and particleboard, and plays the role of a mold and is the core component of the press. The steel belt runs continuously and periodically in a ring form in the press. The steel belt is always subjected to thermal stress caused by temperature changes, tensile stress caused by roller tensioning, and bending stress caused by the bending of the steel belt on the roller surface. In the continuous press, the peak stress of the steel belt is about 500MPa (the sum of tensile stress, thermal stress and bending stress), which requires the stainless steel belt to have high fatigue strength.
[0003] In addition, the roller rod that contacts the inner surface of the steel strip and plays the role of transferring temperature and pressure has a Rockwell hardness of HRC50. When the press is working, there will be sliding friction and rolling friction between the roller rod and the steel strip, and the roller rod will continuously wear the inner surface of the steel strip, which requires the stainless steel strip to have high mechanical properties.
[0004] Therefore, it is necessary to develop a heat treatment process that can improve the performance of stainless steel strip. Summary of the invention
[0005] In view of the above-mentioned problems and needs, the present invention proposes a novel stainless steel strip and a manufacturing method thereof, which solves the above-mentioned problems and brings other technical effects by adopting the following technical features.
[0006] On the one hand, the present invention discloses a method for manufacturing a stainless steel strip, comprising: providing a stainless steel strip having a predetermined size, wherein the stainless steel strip comprises, in weight %, less than 0.09% C, 1%-2% Si, less than 1% Mn, 13.25%-15.25% Cr, 6.5%-7.75% Ni, less than 0.04% P, less than 0.01% S, 0.22%-0.47% Ti, 0.4%-1% Cu, 0.5%-1% Mo, and the balance Fe and unavoidable impurities; and heat treating the stainless steel strip.
[0007] The heat treatment includes: heating to a solution temperature between 1015°C and 1045°C, keeping warm for a first predetermined time, and then cooling to room temperature through a first cooling step; heating to an adjustment temperature between 945°C and 955°C, keeping warm for a second predetermined time, and then cooling to room temperature through a second cooling step; cooling to a cooling temperature less than -80°C, keeping warm for 8 hours; heating to an aging temperature between 505°C and 555°C, keeping warm for 4 hours, and then cooling to room temperature through a third cooling step.
[0008] According to the above embodiments, the stainless steel strip with the composition proposed in the present disclosure is subjected to four steps of solution treatment, adjustment treatment, cold treatment and aging treatment and specific treatment parameter selection to obtain higher fatigue strength and good mechanical properties. The stainless steel strip made according to the manufacturing method proposed in the present disclosure is particularly suitable for the application of stainless steel precision transmission steel strip, and the stainless steel strip is welded end to end to form an annular stainless steel transmission belt.
[0009] In some examples, the first predetermined time is adjusted according to the thickness of the stainless steel strip, and the first predetermined time is between 4 min / mm and 6 min / mm. Preferably, the first predetermined time is 5 min / mm.
[0010] In some examples, the second predetermined time is adjusted according to the thickness of the stainless steel strip, and the first predetermined time is between 8 min / mm and 12 min / mm. Preferably, the second predetermined time is 10 min / mm.
[0011] In some examples, the first cooling step includes cooling with room temperature water. Cooling with room temperature water can quickly cool the stainless steel strip to room temperature.
[0012] In some examples, the second cooling step and / or the third cooling step includes natural cooling in air.
[0013] In some examples, the aging temperature is between 505° C. and 515° C., between 525° C. and 535° C., or between 545° C. and 555° C. The higher the aging temperature, the lower the tensile strength and the higher the fatigue strength, so the appropriate aging temperature can be selected according to the strength requirements of the material.
[0014] In some examples, the cooling process may be performed by liquid nitrogen, for example, cooling in liquid nitrogen to a cooling temperature of less than -80°C.
[0015] On the other hand, the present invention also discloses a stainless steel strip, which contains, by weight%, less than 0.09% C, 1%-2% Si, less than 1% Mn, 13.25%-15.25% Cr, 6.5%-7.75% Ni, less than 0.04% P, less than 0.01% S, 0.22%-0.47% Ti, 0.4%-1% Cu, 0.5%-1% Mo, the remainder Fe and unavoidable impurities, and the stainless steel strip is manufactured by the manufacturing method as described above.
[0016] In some examples, the stainless steel strip has a fatigue strength of ≥570 MPa, a yield strength of ≥1500 MPa, a tensile strength of ≥1550 MPa, and a Rockwell hardness of ≥HRC45.
[0017] Through the heat treatment process disclosed in the present invention, it can be ensured that the fatigue strength of the heat-treated steel strip is not less than 570MPa, the yield strength is ≥1500MPa, the tensile strength is ≥1550MPa, and the Rockwell hardness is ≥HRC45. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present disclosure, but are not intended to limit the present disclosure.
[0019] Figure 1 The metallographic structure (800×) of a stainless steel strip according to at least one embodiment of the present disclosure before heat treatment is shown;
[0020] Figure 2 is a stress-displacement curve diagram of a stainless steel strip according to at least one embodiment of the present disclosure before heat treatment;
[0021] Figure 3 A metallographic structure (800×) diagram of a stainless steel strip according to at least one embodiment of the present disclosure after heat treatment;
[0022] Figure 4 is a stress-displacement curve diagram of a stainless steel strip according to at least one embodiment of the present disclosure after heat treatment;
[0023] Figure 5 A metallographic structure (800×) diagram of a stainless steel strip according to at least one embodiment of the present disclosure before heat treatment;
[0024] Figure 6 is a stress-displacement curve diagram of a stainless steel strip according to at least one embodiment of the present disclosure before heat treatment;
[0025] Figure 7 A metallographic structure (800×) diagram of a stainless steel strip according to at least one embodiment of the present disclosure after heat treatment;
[0026] Figure 8 is a stress-displacement curve diagram of a stainless steel strip according to at least one embodiment of the present disclosure after heat treatment;
[0027] Fig. 9 A metallographic structure (800×) diagram of a stainless steel strip according to at least one embodiment of the present disclosure before heat treatment;
[0028] Fig.10 is a stress-displacement curve diagram of a stainless steel strip according to at least one embodiment of the present disclosure before heat treatment;
[0029] Fig.11 A metallographic structure (800×) diagram of a stainless steel strip according to at least one embodiment of the present disclosure after heat treatment;
[0030] Fig.12 is a stress-displacement curve diagram of a stainless steel strip according to at least one embodiment of the present disclosure after heat treatment;
[0031] Fig.13 FIG. 4 is a curve diagram showing fatigue strength and tensile strength changes of a stainless steel strip according to at least one embodiment of the present disclosure after heat treatment. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the technical solution of the present disclosure clearer, the technical solution of the embodiment of the present disclosure will be clearly and completely described in conjunction with the drawings of the specific embodiments of the present disclosure. It should be noted that the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.
[0033] Unless otherwise defined, the technical or scientific terms used herein shall have the usual meanings understood by persons of ordinary skill in the field to which the present disclosure belongs. The words "first", "second" and similar words used in the patent application specification and claims of the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "a" do not necessarily indicate a quantitative limitation. Words such as "include" or "comprise" mean that the elements, objects or steps that appear before the word include the elements, objects or steps listed after the word and their equivalents, without excluding other elements, objects or steps.
[0034] Stainless steel precision transmission belt is used in continuous hot presses for fiberboard and particleboard, and plays the role of a mold, which is the core component of the press. The steel belt runs continuously and periodically in a ring form in the press. The steel belt is always subjected to thermal stress caused by temperature changes, tensile stress caused by roller tensioning, and bending stress caused by bending of the steel belt on the roller surface. In the continuous press, the peak stress of the steel belt is about 500MPa (the sum of tensile stress, thermal stress and bending stress), which requires the stainless steel transmission belt to have high fatigue strength. In addition, the roller rod that contacts the inner surface of the steel belt and plays the role of temperature and pressure transfer has a Rockwell hardness of HRC50. When the press is working, there will be sliding friction and rolling friction between the roller rod and the steel belt, and the roller rod will continuously wear the inner surface of the steel belt, which requires the stainless steel transmission belt to have high mechanical properties. At present, only one material with the grade of HT1770M can meet such requirements. 14-7PH is a substitute for this material, but with the current heat treatment process, this material cannot have high fatigue strength and mechanical properties at the same time. When running in the press, it is prone to deformation and fatigue cracks caused by roller wear. Therefore, it is necessary to develop a heat treatment process that can improve the performance of 14-7PH.
[0035] The invention discloses a heat treatment process for a grade 14-7PH stainless steel strip. After the heat treatment, the fatigue strength and mechanical properties of the steel strip can reach more than 90% of those of HT1770M, thereby solving the problem that the material is prone to deformation and fatigue cracks when running in a press.
[0036] The present invention discloses a method for manufacturing a stainless steel strip, comprising providing a stainless steel strip having a predetermined size and heat treating the stainless steel strip. The grade 14-7PH stainless steel strip involved in the present disclosure is provided by Outokumpu Press Plate AB of Sweden, and its chemical composition is as follows:
[0037]
[0038] The following describes the role of different elements in the microstructure, the element content is described in weight %, and the ranges described in this disclosure include endpoints:
[0039] Carbon (C) separates the austenite phase and has a strong influence on austenite stability. Up to 0.09% carbon can be added, but higher levels have a detrimental effect on corrosion resistance.
[0040] Silicon (Si) is commonly added to stainless steel for deoxidation purposes in the melt shop, with a maximum of 2.00% and not less than 1.00%.
[0041] Manganese (Mn) is an important additive for stabilizing the austenite phase and increasing the solubility of nitrogen in steel. Thus, manganese can partially replace expensive nickel and bring the steel to a proper phase balance. Too high a level will reduce corrosion resistance. Manganese has a stronger effect on the stability of austenite against deformed martensite than shown in the published literature, and the manganese content must be carefully managed. The range of manganese should be less than 1.00%.
[0042] Chromium (Cr) is the main additive to make steel resistant to corrosion. Chromium ranges from 13.25% to 15.25%.
[0043] Nickel (Ni) is an essential alloying element for achieving good ductility. Ideally, the composition of nickel should be 6.50-7.75%.
[0044] Copper (Cu) is usually present as a residue of 0.4-1.00% in most stainless steels, since the raw material is largely in the form of stainless steel scrap containing this element. Copper is a weak stabilizer of the austenite phase, but has a strong effect on the resistance to martensite formation and must be considered when evaluating the formability of actual alloys. Intentional additions of up to 1.0% may be made.
[0045] Molybdenum (Mo) is a ferrite stabilizer that can be added to increase corrosion resistance. Molybdenum increases resistance to martensite formation, and along with other additives, Mo cannot be added above 1.00%.
[0046] Titanium (Ti) plays a role in making the internal structure of stainless steel dense, refining grain strength, reducing the aging sensitivity of stainless steel, improving the welding performance of stainless steel, increasing the hardness of stainless steel, and increasing the wear resistance and corrosion resistance of stainless steel. The titanium content is preferably controlled in the range of 0.22% to 0.47%.
[0047] In addition, the contents of phosphorus (P) and sulfur (S) also need to be controlled within the range of no more than 0.04% and 0.01%, respectively.
[0048] In this embodiment, the heat treatment includes four steps: solution treatment, adjustment treatment, cold treatment and aging treatment, which are as follows:
[0049] 1. Solution treatment: heating to a solution temperature between 1015°C and 1045°C, holding for a first predetermined time, and then cooling to room temperature through a first cooling step.
[0050] Optionally, the stainless steel strip is solution treated in a resistance furnace in a normal pressure air atmosphere, the solution temperature is 1030°C ± 15°C, the holding time is linearly adjusted according to the thickness of the steel strip, generally 5 min / mm, and then rapidly cooled to room temperature with normal temperature water.
[0051] 2. Conditioning treatment: heating to a conditioning temperature between 945°C and 955°C, keeping the temperature for a second predetermined time, and then cooling to room temperature through a second cooling step.
[0052] Optionally, the stainless steel strip is conditioned by a resistance furnace in a normal pressure air atmosphere, the treatment temperature is adjusted to 950°C ± 5°C, the holding time is linearly adjusted according to the thickness of the steel strip, generally 10 min / mm, and then naturally cooled to room temperature in air, thereby reducing the martensitic transformation points Ms and Mf.
[0053] 3. Cold treatment: Cool to a temperature below -80°C and keep warm for 8 hours.
[0054] Optionally, the cold treatment can be performed by cooling in liquid nitrogen, with the cooling temperature being ≤-80°C and the temperature being kept for 8 hours, so as to obtain sufficient martensite.
[0055] 4. Aging treatment: heating to an aging temperature between 505°C and 555°C, keeping at that temperature for 4 hours, and then cooling to room temperature through a third cooling step.
[0056] By using the aging effect, a dispersed precipitation phase can be produced, thereby further improving the mechanical properties of the steel strip. The aging temperatures are 510℃±5, 530℃±5, and 550℃±5, respectively. The temperature is kept for 4 hours, and then naturally cooled to room temperature in the air. The higher the aging temperature, the lower the tensile strength and the higher the fatigue strength. The fatigue strength and tensile strength change curves at different aging temperatures are shown in Figure 2. Fig.13 .
[0057] The existing heat treatment process only performs aging treatment on the steel strip, and adjusts the fatigue strength of the steel strip by controlling the aging temperature. When the fatigue strength of the steel strip is 550MPa, the yield strength is 1350MPa, the tensile strength is 1400MPa, and the Rockwell hardness is HRC44; through the heat treatment process disclosed in the present invention, it can be ensured that the fatigue strength of the steel strip after heat treatment is not less than 570MPa, the yield strength is ≥1500MPa, the tensile strength is ≥1550MPa, and the Rockwell hardness is ≥HRC45.
[0058] In the case where two or more strips are welded longitudinally to form a wide strip, in a preferred embodiment, a heat treatment is preferably performed prior to welding.
[0059] Examples of preferred embodiments of the stainless steel strip and the method for producing the same according to the present invention are described below.
[0060] Example 1
[0061] First, the metallographic structure and stress displacement curve of 14-7PH are tested, as follows: Figure 1 and Figure 2As shown, a steel strip with a length*width*thickness of 400mm*200mm*3mm is placed in a resistance furnace;
[0062] The first step is solution treatment: heating to 1030℃, keeping warm for 15min, then cooling with normal temperature water to room temperature;
[0063] The second step is adjustment treatment: the steel strip is placed in a resistance furnace, heated to 950°C, kept warm for 30 minutes, and then cooled naturally in the air;
[0064] The third step is cold treatment: place the steel strip in a low temperature box, lower the temperature to -80℃, and keep it warm for 8 hours;
[0065] The fourth step is aging treatment: place the steel strip in a resistance furnace, heat it to 510°C, keep it warm for 4 hours, and cool it with the furnace.
[0066] The test found that granular precipitates appeared between the lath-shaped martensite grains, and the metallographic structure was as follows: Figure 3 As shown, the tensile strength is 1660Mpa and the yield strength is 1600Mpa. Figure 4 As shown, Rockwell hardness HRC49, fatigue strength 580MPa.
[0067] Example 2
[0068] First, the metallographic structure and stress displacement curve of 14-7PH are tested, as follows: Figure 5 and Figure 6 As shown, a steel strip with a length*width*thickness of 400mm*200mm*3mm is placed in a resistance furnace;
[0069] The first step is solution treatment: heating to 1030℃, keeping warm for 15min, then cooling with normal temperature water to room temperature;
[0070] The second step is adjustment treatment: the steel strip is placed in a resistance furnace, heated to 950°C, kept warm for 30 minutes, and then cooled naturally in the air;
[0071] The third step is cold treatment: place the steel strip in a low temperature box, lower the temperature to -80℃, and keep it warm for 8 hours;
[0072] The fourth step is aging treatment: place the steel strip in a resistance furnace, heat it to 530°C, keep it warm for 4 hours, and cool it with the furnace.
[0073] The test found that granular precipitates appeared between the lath-shaped martensite grains, and the metallographic structure was as follows: Figure 7 As shown, the tensile strength is 1560Mpa and the yield strength is 1500Mpa. Figure 8 As shown, Rockwell hardness HRC46, fatigue strength 600MPa.
[0074] Example 3
[0075] First, the metallographic structure and stress displacement curve of 14-7PH are tested, as follows: Fig. 9 and Fig.10 As shown, a steel strip with a length*width*thickness of 400mm*200mm*2mm is placed in a resistance furnace;
[0076] The first step is solution treatment: heating to 1030℃, keeping warm for 10min, then cooling with room temperature water to room temperature;
[0077] The second step is adjustment treatment: the steel strip is placed in a resistance furnace, heated to 950°C, kept warm for 20 minutes, and then cooled naturally in the air;
[0078] The third step is cold treatment: place the steel strip in a low temperature box, lower the temperature to -80℃, and keep it warm for 8 hours;
[0079] The fourth step is aging treatment: place the steel strip in a resistance furnace, heat it to 550°C, keep it warm for 4 hours, and cool it with the furnace.
[0080] The test found that granular precipitates appeared between the lath-shaped martensite grains, and the metallographic structure was as follows: Fig.11 As shown, the tensile strength is 1440Mpa and the yield strength is 1400Mpa. Fig.12 As shown, Rockwell hardness HRC43, fatigue strength 630MPa.
[0081] In particular, individual embodiments can form the subject matter of independent solutions according to the invention.
[0082] The exemplary implementation of the metal transmission belt and the manufacturing method thereof proposed in the present disclosure is described in detail with reference to the preferred embodiments. However, it can be understood by those skilled in the art that various modifications and variations can be made to the above specific embodiments without departing from the concept of the present disclosure. In addition, various technical features, structures or steps proposed in various aspects of the present disclosure can also be combined in various ways without exceeding the protection scope of the present disclosure, which is determined by the attached claims.
Claims
1. A method for manufacturing a stainless steel strip, include: A stainless steel strip having a predetermined size is provided, wherein the stainless steel strip comprises, in weight %, less than 0.09% C, 1%-2% Si, less than 1% Mn, 13.25%-15.25% Cr, 6.5%-7.75% Ni, less than 0.04% P, less than 0.01% S, 0.22%-0.47% Ti, 0.4%-1% Cu, 0.5%-1% Mo, and the balance Fe and unavoidable impurities; The stainless steel strip is subjected to heat treatment, wherein the heat treatment comprises: Heating to a solution temperature between 1015°C and 1045°C, holding for a first predetermined time, and then cooling to room temperature via a first cooling step; heating to an adjusted temperature between 945°C and 955°C, maintaining the temperature for a second predetermined time, and then cooling to room temperature via a second cooling step; Cool to a cooling temperature less than -80°C and keep warm for 8 hours; Heating to an aging temperature between 525°C and 535°C or between 545°C and 555°C, maintaining the temperature for 4 hours, and then cooling to room temperature through a third cooling step, The first predetermined time is adjusted according to the thickness of the stainless steel strip, and the first predetermined time is between 4 min / mm and 6 min / mm. Wherein, the second predetermined time is adjusted according to the thickness of the stainless steel strip, and the second predetermined time is 10 min / mm.
2. The manufacturing method according to claim 1, in, The first predetermined time is 5 min / mm.
3. The manufacturing method according to claim 1, in, The first cooling step includes cooling using room temperature water.
4. The manufacturing method according to claim 1, in, The second cooling step and / or the third cooling step comprises natural cooling in air.
5. The manufacturing method according to claim 1, in, Cool in liquid nitrogen to a cooling temperature of less than -80°C.
6. A stainless steel strip, comprising, in weight %, less than 0.09% C, 1%-2% Si, less than 1% Mn, 13.25%-15.25% Cr, 6.5%-7.75% Ni, less than 0.04% P, less than 0.01% S, 0.22%-0.47% Ti, 0.4%-1% Cu, 0.5%-1% Mo, the balance Fe and unavoidable impurities, the stainless steel strip being manufactured by the manufacturing method according to any one of claims 1 to 5.
7. The stainless steel strip according to claim 6, in, The fatigue strength of the stainless steel strip is ≥570MPa, the yield strength is ≥1500MPa, the tensile strength is ≥1550MPa, and the Rockwell hardness is ≥HRC45.