A kind of superfine fiber leather soap fastness improving agent and preparation method thereof

By synthesizing a combination of polyquaternium copolymers and modified cyclodextrin derivatives, the problems of poor dyeing performance and insufficient soaping fastness of nylon microfiber leather are solved, and efficient low-temperature soaping effects are achieved to meet the needs of the market 3 Grade soaping fastness requirements and improved stability and friction properties.

CN116024831BActive Publication Date: 2024-10-11SHANGHAI YAYUN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211724660.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-11
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Nylon microfiber leather has poor dyeing performance and insufficient soaping fastness, making it unable to meet market requirements for level 3 or above. The existing soaping agent transfer and complex preparation processes are deficient.

Method used

A low-temperature soaping fastness enhancer is prepared by synthesizing the reaction of epoxy-containing compounds, amino-containing compounds and imidazole-containing compounds to generate polyquaternary ammonium salt copolymers, and mixing them with modified cyclodextrin derivatives and emulsifiers. , using specific process conditions to carry out intermolecular dehydration reaction to form a stable polyquaternary ammonium salt copolymer.

Benefits of technology

It significantly improves the soaping fastness of nylon microfiber leather, reaching market level 3 requirements, and improves the stability and rubbing fastness of the product, especially in wet rubbing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004029171150000021
    Figure BDA0004029171150000021
  • Figure BDA0004029171150000031
    Figure BDA0004029171150000031
  • Figure BDA0004029171150000032
    Figure BDA0004029171150000032
Patent Text Reader

Abstract

The invention discloses a microfiber leather soap fastness improver and a preparation method thereof. The soap fastness improver of the invention comprises the following components: 65-91 weight percent of a modified cationic polyquaternary ammonium compound, 3-18 weight percent of a modified cyclodextrin derivative, 5-28 weight percent of an emulsifier, and 0.1-5 weight percent of a dispersant, based on the total weight of the microfiber leather soap fastness improver. The soap fastness improver of the invention has good soap fastness improvement under low temperature conditions of 40-50° C., and has excellent performances of removing floating color and improving color fastness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile auxiliaries, and in particular to an ultrafine fiber leather soaping fastness improving agent and a preparation method thereof. Background Art

[0002] Natural leather has always been loved by people. However, resources are limited, so it is necessary to develop synthetic leather with excellent performance. At present, microfiber synthetic leather (abbreviated as microfiber leather) is the most ideal material to replace natural leather and is widely used in many industries. Microfiber synthetic leather is similar to natural leather, and some properties such as physical and mechanical properties are even better than natural leather. Due to the small number of hydrophilic groups on the microfiber base fabric, its dyeing performance is still far behind that of natural leather.

[0003] At present, most of the domestic leather is made of nylon microfiber. Due to its special structure, nylon microfiber leather fiber has poor dyeability. A higher dye concentration is required for dyeing, generally 4-8% (owf), and some are even as high as 20%. However, most of these dyes are only adsorbed on the surface of nylon microfiber leather, and the binding force with nylon microfiber leather is relatively weak, so the color fastness of nylon microfiber leather is poor. After dyeing, it is necessary to thoroughly wash or soap at a low temperature of 40-50℃ to remove surface floating color and unfixed dyes. The market requires at least level 3 soap fastness for microfiber leather, but the current level is generally level 1-2, which is far from meeting market requirements.

[0004] The development of nylon microfiber leather soap fastness enhancer that meets market requirements has a broad market and is a future development trend. The simplest idea is to transfer the application, such as transferring the nylon soaping agent to nylon microfiber leather. The literature on nylon soaping fastness enhancer that has been disclosed, such as patent publication number CN110552217A discloses a nylon fixed color spot preventer, in which various surfactants are added to prevent the generation of fixed color spots, but its soaping performance is weak. For example, patent publication number CN113529444A discloses a white bottom anti-staining soaping fastness enhancer for nylon, which is prepared by reacting fatty amine polyoxyethylene ether quaternary ammonium salt, maleic anhydride, acrylic acid and N-vinyl pyrrolidone to obtain a copolymer, but its preparation process is relatively cumbersome, and the soaping temperature needs to be 85-95°C. The inventors also experimented with applying the nylon soaping agent in the above patent to nylon microfiber leather at 40-50°C, and found that the soaping fastness improvement was poor.

[0005] The inventors have conducted an in-depth study on the relationship between structure and performance, and prepared a low-temperature soap fastness enhancer with excellent performance through reasonable molecular structure design. Summary of the invention

[0006] The object of the present invention is to provide a microfiber leather soap fastness improving agent with stable performance, energy saving and high efficiency and a preparation method thereof.

[0007] One aspect of the present invention provides a microfiber leather soap fastness enhancer, which comprises the following components:

[0008]

[0009] The total weight of the microfiber leather is used as a basis.

[0010] Another aspect of the present invention provides a method for preparing a microfiber leather soap fastness improving agent, which comprises the following steps:

[0011] a) completely dissolving the epoxy compound b of formula (II) and the amino compound c of formula (III) in benzyl alcohol, reacting for 2-4 hours, removing the benzyl alcohol, and generating the addition compound e of formula (V); completely dissolving the epoxy compound b of formula (II) and the imidazole compound d of formula (IV) in toluene, reacting for 4-8 hours at 80-90° C., in the presence of an inert gas and a catalyst, and adjusting the pH value to 7-8, to generate the quaternary ammonium compound f of formula (VI); adding the addition compound e of formula (V) and the quaternary ammonium compound f of formula (VI) to dimethyl sulfoxide, and carrying out an intermolecular dehydration reaction at 130-150° C. for 0.5-2 hours under the catalysis of concentrated sulfuric acid, to generate the polyquaternary ammonium salt copolymer a of formula (I);

[0012] b) uniformly mixing a dispersant, an emulsifier, a modified cyclodextrin derivative and the polyquaternary ammonium salt copolymer a of formula (I) synthesized in a) at a mass ratio of 1: (5-180): (3-180): (65-300),

[0013]

[0014] Formula (I)

[0015]

[0016] Formula (II)

[0017]

[0018] Formula (III)

[0019]

[0020] Formula (IV)

[0021]

[0022] Formula (V)

[0023]

[0024] Formula (VI)

[0025] R1 and R2 are each independently selected from H, -(CH2)nCH3, halogen, glycidyl ether, wherein n is an integer of 0-5;

[0026] R3 is -CH2CH2(CH2CH2NH)m or phenylene, wherein m is an integer from 0 to 5;

[0027] R4 is oleyl, coconut oil or -(CH2)pCH3, wherein p is an integer of 11-17;

[0028] q is an integer from 10 to 20. DETAILED DESCRIPTION

[0029] In one embodiment, the microfiber leather soap fastness improving agent of the present invention comprises the following components:

[0030]

[0031] The total weight of the microfiber leather soap fastness enhancer is used as a benchmark.

[0032] Preferably, the modified polyquaternary ammonium salt copolymer is a polyquaternary ammonium salt copolymer a represented by formula (I),

[0033]

[0034] Formula (I)

[0035] R1 and R2 are each independently selected from H, -(CH2)nCH3, halogen, glycidyl ether, wherein n is an integer of 0-5;

[0036] R3 is -CH2CH2(CH2CH2NH)m or phenylene, wherein m is an integer from 0 to 5;

[0037] R4 is oleyl, coconut oil or -(CH2)pCH3, wherein p is an integer of 11-17;

[0038] q is an integer from 10 to 20.

[0039] Preferably, the polyquaternary ammonium salt copolymer a is prepared by an addition reaction of an epoxy-containing compound b represented by formula (II) and an amino-containing compound c represented by formula (III) to generate an addition compound e represented by formula (V), and a quaternary ammonium compound f represented by formula (VI) is prepared by a quaternary amination reaction of an epoxy-containing compound b represented by formula (II) and an imidazole-containing compound d represented by formula (IV), and then the addition compound e represented by formula (V) and the quaternary ammonium compound f represented by formula (VI) undergo intermolecular dehydration to generate:

[0040]

[0041] Formula (II)

[0042]

[0043] Formula (III)

[0044]

[0045] Formula (IV)

[0046]

[0047] Formula (V)

[0048]

[0049] Formula (VI).

[0050] Preferably, the epoxy-containing compound b shown in formula (II) is selected from one or more of ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, diglycidyl ether, and diethylene glycol diglycidyl ether; the amino-containing compound c shown in formula (III) is selected from one or more of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, hexaethyleneheptamine, and phenylenediamine; the imidazole-containing compound d shown in formula (IV) is selected from one or more of oleyl hydroxyethyl imidazoline, coconut oil hydroxyethyl imidazoline, and lauryl hydroxyethyl imidazoline.

[0051] Preferably, the molecular weight of the quaternary ammonium compound f represented by formula (VI) is 800-2000, and the molecular weight of the polyquaternary ammonium salt copolymer a represented by formula (I) is 2000-5000.

[0052] Preferably, the weight ratio of the epoxy-containing compound b shown in formula (II) to the amino-containing compound c shown in formula (III) is (1.0-2.2):1, the weight ratio of the epoxy-containing compound b shown in formula (II) to the imidazole-containing compound d shown in formula (IV) is (2.0-4.0):1, and the weight ratio of the addition compound e shown in formula (V) to the quaternary ammonium compound f shown in formula (VI) is 1:(0.4-1.2).

[0053] Preferably, the modified cyclodextrin derivative is selected from one or more polymers generated by the reaction of C1-3 cyclodextrin and epichlorohydrin.

[0054] Preferably, the dispersant is selected from one or more of polyvinyl pyrrolidones and maleic acid-acrylic acid copolymers.

[0055] Preferably, the emulsifier is selected from one or more of fatty alcohol acid amines, fatty imidazoline salts, fatty dihydroxyethyl amine oxides, long-chain alkyl dimethyl betaine, fatty amides, and fatty amino acid imidazolines.

[0056] According to one embodiment of the present invention, there is provided a method for preparing a microfiber leather soap fastness improving agent, which comprises the following steps:

[0057] a) completely dissolving the epoxy-containing compound b of formula (II) and the amino-containing compound c of formula (III) in benzyl alcohol, reacting for 2-4 hours, removing the benzyl alcohol, and generating the addition compound e of formula (V); completely dissolving the epoxy-containing compound b of formula (II) and the imidazole-containing compound d of formula (IV) in toluene, reacting for 4-8 hours at 80-90° C., under the protection of an inert gas such as N2 and a catalyst, and adjusting the pH value to 7-8, to generate the quaternary ammonium compound f of formula (VI); adding the addition compound e of formula (V) and the quaternary ammonium compound f of formula (VI) to dimethyl sulfoxide, and carrying out an intermolecular dehydration reaction at 130-150° C. for 0.5-2 hours under the catalysis of concentrated sulfuric acid, to generate the polyquaternary ammonium salt copolymer a of formula (I);

[0058] b) uniformly mixing a dispersant, an emulsifier, a modified cyclodextrin derivative and the polyquaternary ammonium salt copolymer a of formula (I) synthesized in a) in a mass ratio of 1:(5-180):(3-180):(65-300).

[0059] The invention can control the performance index of the mixture by adjusting the mass ratio, the product is not easy to hydrolyze, and the appearance and structural stability are improved.

[0060] Example

[0061] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0062] The basic chemicals, general industrial chemicals and ultrafine fiber leather used in the present invention are all commonly available on the market.

[0063] The performance of the microfiber leather soap fastness enhancer prepared in each embodiment of the present invention is verified by the following tests.

[0064] Microfiber leather performance test

[0065] 1. Fabric: Dyed nylon microfiber leather

[0066] 2. Process and dosage

[0067] Soap fastness enhancer: 20g / L

[0068] One dip and one roll (liquid rate 45-50%) → drying (120℃*2min) → 40-50℃ soap washing → 30-40℃ warm water washing → room temperature water washing → drying (70-80℃)

[0069] 3. Performance Testing

[0070] 3.1 Stability

[0071] Place the product in a sealed sample bottle at 25°C for 6 months and observe whether the product is stratified or precipitated.

[0072] 3.2 Soap fastness

[0073] Refer to GB / T 3921-2008, C(3) to measure soap fastness, single fiber lining, the larger the value, the better the soaping effect.

[0074] 3.3 Rubbing fastness

[0075] Dry and wet friction fastness: According to GB / T 3920-2008, tested by friction fastness tester, the higher the rating, the better the dry and wet friction resistance.

[0076] 3.4 Molecular weight determination

[0077] The molecular weight was measured using a gel chromatography instrument Breeze GPC (Waters).

[0078] Example 1

[0079] 1) 0.136 parts by weight of ethylenediamine (industrial grade, Shanghai Zhongcheng Chemical Co., Ltd.), 20 parts by weight of benzyl alcohol (industrial grade), and 0.168 parts by weight of butylene oxide (industrial grade) were completely dissolved in a three-necked flask, and the mixture was reacted for 4 hours at room temperature. After the reaction was complete, the benzyl alcohol was removed by low-pressure distillation (13 Pa) and the mixture was set aside. 0.694 parts by weight of butylene oxide and 0.284 parts by weight of oleyl hydroxyethyl imidazoline were added to 30 parts by weight of toluene and completely dissolved, and the mixture was reacted for 4 hours at 85°C under N2 protection and under the action of Y molecular sieve NaY (Zhoran Environmental Protection Technology (Dalian) Co., Ltd.), and the pH value was adjusted to 7.4 and the mixture was set aside. 0.289 parts by weight of the addition compound e represented by formula (V) and 0.176 parts by weight of the quaternary ammonium compound f represented by formula (VI) (molecular weight 1400) were added to 20 parts by weight of DMSO solvent, and reacted at 140° C. for 0.5 h under the catalysis of concentrated sulfuric acid to generate a modified polyquaternary ammonium salt copolymer a-1 (molecular weight 3000) for later use.

[0080] 2) Under the action of 10 parts by weight of coconut dihydroxyethyl amine oxide (industrial grade, Hai'an Petrochemical, Jiangsu Province) as an emulsifier, 1 part by weight of polyvinyl pyrrolidone, 6 parts by weight of a polymer generated by the reaction of hydroxymethyl cyclodextrin and epichlorohydrin (industrial grade, Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.) and 90 parts by weight of the above-mentioned modified polyquaternary ammonium salt copolymer a-1 are uniformly mixed to obtain a microfiber leather soap fastness enhancer.

[0081] Example 2

[0082] 1) 0.186 parts by weight of triethylenetetramine (industrial grade, Shanghai Zhongcheng Chemical Co., Ltd.), 30 parts by weight of benzyl alcohol (industrial grade), and 0.218 parts by weight of glycidyl ether (industrial grade, Tianjin Yuanli Chemical Co., Ltd.) were completely dissolved in a three-necked flask, and reacted for 4 hours at room temperature. After the reaction was complete, the benzyl alcohol was removed by low-pressure distillation (13 Pa) and set aside. 0.654 parts by weight of glycidyl ether and 0.318 parts by weight of lauryl hydroxyethyl imidazoline were added to 30 parts by weight of toluene and completely dissolved, and reacted for 4 hours at 85°C under N2 protection and under the action of Y molecular sieve NaY, and the pH value was adjusted to 7.8 and set aside. 0.369 parts by weight of the addition compound e represented by formula (V) and 0.295 parts by weight of the quaternary ammonium compound f represented by formula (VI) (molecular weight 1800) were added to 50 parts by weight of DMSO solvent, and reacted at 140° C. for 1 hour under the catalysis of concentrated sulfuric acid to generate a modified polyquaternary ammonium salt copolymer a-2 (molecular weight 4200) for later use.

[0083] 2) Under the action of 15 parts by weight of hexadecyl dimethyl betaine (industrial grade, Hai'an Petrochemical, Jiangsu Province) as an emulsifier, 1 part by weight of maleic acid-acrylic acid copolymer, 6 parts by weight of a polymer generated by the reaction of hydroxyethyl cyclodextrin and epichlorohydrin (industrial grade, Hubei Jiangmin Taihua Chemical Co., Ltd.) and 85 parts by weight of the above-generated modified polyquaternary ammonium salt copolymer a-2 are uniformly mixed to obtain a microfiber leather soap fastness enhancer.

[0084] Example 3

[0085] 1) 0.163 parts by weight of phenylenediamine (industrial grade, Shanghai Zhongcheng Chemical Co., Ltd.), 25 parts by weight of benzyl alcohol (industrial grade), and 0.198 parts by weight of propylene oxide (industrial grade, Tianjin Yuanli Chemical Co., Ltd.) were completely dissolved in a three-necked flask, and reacted for 4 hours at room temperature. After the reaction was complete, the benzyl alcohol was removed by low-pressure distillation (13 Pa) and set aside. 0.798 parts by weight of propylene oxide and 0.324 parts by weight of coconut oil hydroxyethyl imidazoline were added to 40 parts by weight of toluene and completely dissolved, and reacted for 4 hours at 85°C under N2 protection and under the action of Y molecular sieve NaY, and the pH value was adjusted to 7.5 and set aside. 0.349 parts by weight of the addition compound e represented by formula (V) and 0.246 parts by weight of the quaternary ammonium compound f represented by formula (VI) (molecular weight 1200) were added to 40 parts by weight of DMSO solvent, and reacted at 145° C. for 1 hour under the catalysis of concentrated sulfuric acid to generate a modified polyquaternary ammonium salt copolymer a-3 (molecular weight 2700) for later use.

[0086] 2) Under the action of 20 parts by weight of coconut oil fatty acid diethanolamide (industrial grade, Hai'an Petrochemical, Jiangsu Province), an emulsifier, 1 part by weight of polyvinyl pyrrolidone, 10 parts by weight of a polymer generated by the reaction of hydroxypropyl cyclodextrin and epichlorohydrin (industrial grade, Xi'an Qiyue Biotechnology Co., Ltd.) and 82 parts by weight of the above-mentioned modified polyquaternary ammonium salt copolymer a-3 are uniformly mixed to obtain a microfiber leather soap fastness enhancer.

[0087] The performance effects of various embodiments are shown in Table 1.

[0088] Table 1 Comparison of application effects of different nylon microfiber leather soap fastness enhancers

[0089]

[0090] Note: The soap fastness of the original microfiber leather is level 1-2; the dry rubbing fastness is level 3, and the wet rubbing fastness is level 1-2.

[0091] As can be seen from Table 1, the product of the present invention significantly improves the soap washing fastness of microfiber leather, can meet the requirements of market level 3, has good stability, excellent dry and wet rubbing fastness, especially wet rubbing fastness, which is higher than level 1 of market products.

[0092] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the protection scope of the present invention. Any changes and modifications made by any technician familiar with the technology without departing from the concept and scope of the present invention should fall within the protection scope of the present invention.

Claims

1. A superfine fiber leather soap fastness enhancer, comprising the following components: Based on the total weight of the microfiber leather soap fastness enhancer, The modified polyquaternary ammonium salt copolymer is a polyquaternary ammonium salt copolymer a represented by formula (I), R1 and R2 are each independently selected from H, -(CH2)nCH3, halogen, glycidyl ether, wherein, n is an integer from 0 to 5; R3 is -CH2CH2(CH2CH2NH)m- or phenylene, wherein m is an integer from 0 to 5; R4 is oleyl, coconut oil or -(CH2)pCH3, wherein p is an integer of 11-17; q is an integer between 10 and 20, The modified cyclodextrin derivative is selected from one or more polymers generated by the reaction of C1-3 cyclodextrin and epichlorohydrin.

2. The microfiber leather soap fastness improving agent according to claim 1, characterized in that: The polyquaternary ammonium salt copolymer a is prepared by an addition reaction between an epoxy-containing compound b represented by formula (II) and an amino-containing compound c represented by formula (III) to generate an addition compound e represented by formula (V), a quaternary ammonium compound f represented by formula (VI) is prepared by a quaternary amination reaction between an epoxy-containing compound b represented by formula (II) and an imidazole-containing compound d represented by formula (IV), and then the addition compound e represented by formula (V) and the quaternary ammonium compound f represented by formula (VI) undergo intermolecular dehydration to generate:

3. The soap fastness improving agent for microfiber leather according to claim 2, characterized in that: The epoxy-containing compound b shown in formula (II) is selected from one or more of ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, diglycidyl ether, and diethylene glycol diglycidyl ether; the amino-containing compound c shown in formula (III) is selected from one or more of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, hexaethyleneheptamine, and phenylenediamine; the imidazole-containing compound d shown in formula (IV) is selected from one or more of oleyl hydroxyethyl imidazoline, coconut oil hydroxyethyl imidazoline, and lauryl hydroxyethyl imidazoline.

4. The soap fastness improving agent for microfiber leather according to claim 2, characterized in that: The molecular weight of the quaternary ammonium compound f represented by formula (VI) is 800-2000, and the molecular weight of the polyquaternary ammonium salt copolymer a represented by formula (I) is 2000-5000.

5. The microfiber leather soap fastness improving agent according to claim 2, characterized in that: The weight ratio of the epoxy-containing compound b shown in formula (II) to the amino-containing compound c shown in formula (III) is (1.0-2.2):1, the weight ratio of the epoxy-containing compound b shown in formula (II) to the imidazole-containing compound d shown in formula (IV) is (2.0-4.0):1, and the weight ratio of the addition compound e shown in formula (V) to the quaternary ammonium compound f shown in formula (VI) is 1:(0.4-1.2).

6. The microfiber leather soap fastness improving agent according to claim 1, characterized in that: The dispersant is selected from one or more of polyvinyl pyrrolidones and maleic acid-acrylic acid copolymers.

7. The soap fastness improving agent for microfiber leather according to claim 1, characterized in that: The emulsifier is selected from one or more of fatty alcohol acid amines, fatty imidazoline salts, fatty dihydroxyethyl amine oxides, long-chain alkyl dimethyl betaine, fatty amides, and fatty amino acid imidazolines.

8. A method for preparing the microfiber leather soap fastness improving agent according to any one of claims 1 to 7, comprising the following steps: a) completely dissolving the epoxy compound b of formula (II) and the amino compound c of formula (III) in benzyl alcohol, reacting for 2-4 hours, removing the benzyl alcohol, and generating the addition compound e of formula (V); completely dissolving the epoxy compound b of formula (II) and the imidazole compound d of formula (IV) in toluene, reacting for 4-8 hours at 80-90° C., in the presence of an inert gas and a catalyst, and adjusting the pH value to 7-8, to generate the quaternary ammonium compound f of formula (VI); adding the addition compound e of formula (V) and the quaternary ammonium compound f of formula (VI) to dimethyl sulfoxide, and carrying out an intermolecular dehydration reaction at 130-150° C. for 0.5-2 hours under the catalysis of concentrated sulfuric acid, to generate the polyquaternary ammonium salt copolymer a of formula (I); b) uniformly mixing a dispersant, an emulsifier, a modified cyclodextrin derivative and the polyquaternary ammonium salt copolymer a of formula (I) synthesized in a) at a mass ratio of 1: (5-180): (3-180): (65-300), R1 and R2 are each independently selected from H, -(CH2)nCH3, halogen, glycidyl ether, wherein, n is an integer from 0 to 5; R3 is -CH2CH2(CH2CH2NH)m or phenylene, wherein m is an integer from 0 to 5; R4 is oleyl, coconut oil or -(CH2)pCH3, wherein p is an integer of 11-17; q is an integer of 10-20.