Hydroisomerization catalyst and preparation method thereof and hydrocarbon oil hydroisomerization treatment method
By using the ellipsoid-shaped ZSM-48 molecular sieve and the active metal hydrogenation isomerization catalyst, the problem of low product yield of the hydrogenation isomerization catalyst in the existing technology is solved, achieving higher product yield and lower The freezing point improves the production efficiency of lubricants.
Patent Information
- Application Number
- CN202111261637.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Existing hydroisomerization catalysts have low product yields in catalytic reactions, which affects the production efficiency of lubricating oil products.
A hydrogenation isomerization catalyst containing ZSM-48 molecular sieve with ellipsoidal morphology is used. The specific surface area and grain size of ZSM-48 molecular sieve are controlled through a specific preparation method, and active metals are introduced by impregnation method to improve catalytic performance.
It significantly increases the product yield and viscosity index of the hydroisomerization reaction, reduces the freezing point of the product, and improves the efficiency and performance of the catalyst.
Smart Images

Figure CN116037201B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalysts, and in particular to a hydroisomerization catalyst and a preparation method thereof, and a hydrocarbon oil hydroisomerization treatment method. Background Art
[0002] When using raw oil with a high content of paraffins to produce low-freezing diesel or lubricating oil base oil, dewaxing treatment is required to reduce the freezing point and improve the low-temperature fluidity of the product. Isomerization of paraffins in the presence of a hydroisomerization catalyst can significantly improve the low-temperature fluidity of the oil while maintaining a suitable viscosity. The carrier material of the hydroisomerization catalyst usually contains different types of molecular sieves. The molecular sieve material has high acidity and high specific surface area and is an excellent acid catalyst. At the same time, the molecular sieve material has strong chemical stability and hydrothermal stability, and it is difficult to be corroded and dissolved by the reactants and destroyed. Compared with the commonly used homogeneous catalysts, the molecular sieve material catalyst can be directly reused without separation, and will not cause pollution to the environment and products.
[0003] CN104353484A discloses a method for preparing a cheap strongly acidic multi-level pore Beta zeolite, and relates to a method for preparing a multi-level pore Beta zeolite. The invention aims to solve the problem of weakened acidity of the existing multi-level pore Beta zeolite molecular sieve after desiliconization. The method comprises: (1) calcining Beta zeolite to obtain microporous hydrogen-type Beta zeolite; (2) adding the microporous hydrogen-type Beta zeolite to an alkaline solution, stirring, washing, and drying to obtain a sodium-type desiliconized multi-level pore Beta zeolite; (3) adding the sodium-type desiliconized multi-level pore Beta zeolite to an ammonium nitrate aqueous solution for exchange, and obtaining a hydrogen-type desiliconized multi-level pore Beta zeolite after calcination; (4) adding the hydrogen-type desiliconized multi-level pore Beta zeolite to an acid solution, stirring, washing, and drying, and then repeating step (3) to obtain a strongly acidic multi-level pore Beta zeolite.
[0004] CN103073020A discloses a multi-level pore zeolite molecular sieve and its preparation method and application. The preparation method is specifically: using a cationic surfactant as a template, assembling silanized zeolite seeds under hydrothermal conditions, and preparing a method for preparing a multi-level pore zeolite molecular sieve. This method overcomes the problem that the multi-level pore zeolite cannot be prepared due to the mismatch between conventional cationic surfactants and zeolite templates. The prepared material realizes the composite of micropores and mesopores, and is a multi-level pore zeolite molecular sieve with high crystallization. However, this method essentially utilizes a specific functional group reaction to graft organosilane to the seed, and cooperates with a cationic surfactant to prepare a mesoporous molecular sieve. In this process, the formation of mesopores is guided by the cationic surfactant, and the hard template effect of the organosilane is used to form mesopores with a pore size of about 2.4nm. The seed crystal selected in this invention is a microporous molecular sieve, which is added to the preparation system after silanization. Its hydrophobicity is used to increase its effect on the hydrophobic end of the surfactant micelle, thereby reducing the interaction between the two directing agents. However, the formed mesopores still do not have a regular structure, and there is no report on whether the addition of the seed crystal reduces the amount of template used.
[0005] CN102245294B discloses a method for dewaxing a hydrocarbon feedstock containing a waxy component, the method comprising contacting the feedstock with a catalyst system comprising ZSM-48 and MTT framework structure type molecular sieves under dewaxing conditions. The ZSM-48 has a silicon dioxide to aluminum oxide molar ratio of less than 100, wherein the MTT framework structure type molecular sieve has a silicon dioxide to aluminum oxide molar ratio of less than 45, wherein the MTT framework structure type molecular sieve is ZSM-23, and wherein the ratio of ZSM-48 to ZSM-23 is at least 75:25. The ZSM-48 type molecular sieve is a new type of high-silicon molecular sieve developed in the 1980s, having a two-dimensional ten-membered ring channel structure, belonging to the orthorhombic system, the channels are connected by 5-membered rings, and the orifice diameter is about 0.6nm. It is characterized by a higher silicon aluminum molar ratio and a tubular linear channel, which can accommodate organic molecules with a kinetic radius smaller than benzene. Theoretically, ZSM-48 molecular sieve has a smaller pore "self-impedance effect", and the pore size is suitable for the shape-selective isomerization of chain alkanes. At present, many synthesis methods of ZSM-48 molecular sieves have been reported at home and abroad.
[0006] CN101801848A discloses a method for preparing ZSM-48, comprising: (a) providing an aqueous reaction mixture comprising at least one silica source, at least one alumina source, at least one hydroxyl ion source, at least one alkyl diquaternary ammonium source R 2+ , having the formula (CH3)3N + (CH3)3 ions, and optionally seeds, wherein the composition of the reaction mixture comprises the following molar ratios: R 2+:SiO2 is less than 0.1, SiO2:Al2O3 is less than 100, OH - : SiO2 is less than 0.2; and (b) crystallizing the reaction mixture under conditions effective to prepare the ZSM-48.
[0007] CN102910642A discloses a method for preparing a ZSM-48 molecular sieve, comprising: (1) mixing a silicon source, an aluminum source, an alkali, water and a template agent uniformly, and expressing the molar ratio composition in terms of oxides: DBH / SiO2=0.025-0.20, TMA / SiO2=0.05-0.40, ETA / SiO2=0.25-1.50, SiO2 / Al2O3=150-500, Na2O / SiO2=0.01-0.20, H2O / SiO2=5-50, DBH represents the template agent dibromohexane; TMA represents the template agent blue methylamine; ETA represents the template agent ethanol; (2) crystallization: heating the reaction mixture to 150-170°C and hydrothermally crystallizing for 4-10 days; (3) after the crystallization is completed, filtering, washing and drying to obtain the ZSM-48 molecular sieve. The method uses a relatively cheap template to synthesize a ZSM-48 molecular sieve with a low silicon-aluminum ratio for use in hydroisomerization dewaxing.
[0008] In summary, in the existing technology, the product yield of hydroisomerization dewaxing still has room for improvement. Therefore, it is crucial to develop new hydroisomerization catalysts and matching processes to improve the efficiency of lubricant production. Summary of the invention
[0009] The purpose of the present invention is to overcome the problem of low product yield of hydroisomerization catalysts used in catalytic reactions in the prior art, and to provide a hydroisomerization catalyst and a preparation method thereof, as well as a hydrocarbon oil hydroisomerization treatment method. The hydroisomerization catalyst contains a ZSM-48 molecular sieve, which has an ellipsoidal morphology and a large specific surface area. The hydroisomerization catalyst has excellent catalytic performance in hydrocarbon oil hydroisomerization reactions.
[0010] In order to achieve the above object, the present invention provides a hydroisomerization catalyst, which comprises a carrier and an active metal supported on the carrier, wherein the carrier comprises a ZSM-48 molecular sieve, wherein the molar ratio of silicon oxide to aluminum oxide in the ZSM-48 molecular sieve is not less than 40, and the specific surface area of the ZSM-48 molecular sieve is not less than 200 m 2 / g, the ZSM-48 molecular sieve has an ellipsoidal grain shape, a major diameter not exceeding 700nm and an aspect ratio of 1-3:1;
[0011] The active metal is selected from at least one of Pt, Pd, Ni and Co.
[0012] The second aspect of the present invention provides a method for preparing the hydroisomerization catalyst described in the first aspect, which comprises mixing the ZSM-38 molecular sieve with an optional binder and / or a binder precursor, and then optionally molding and drying to obtain a carrier, and then introducing an active metal into the carrier by an impregnation method.
[0013] The third aspect of the present invention provides a method for hydroisomerization treatment of hydrocarbon oil, comprising: under hydroisomerization conditions, contacting a feedstock oil with a hydroisomerization catalyst, wherein the feedstock oil is selected from at least one of cracking tail oil, bio-jet fuel production feedstock, C5C6 isomerization feedstock, and Fischer-Tropsch synthesis wax, and the hydroisomerization catalyst is the hydroisomerization catalyst described in the first aspect.
[0014] Through the above technical scheme, the hydroisomerization catalyst provided by the present invention contains a ZSM-48 molecular sieve with an ellipsoidal morphology, and the molecular sieve has a molecular sieve having a molecular weight of not less than 200 m 2 / g specific surface area, and when the hydroisomerization catalyst is used for the hydroisomerization of waxy oil, the product yield and viscosity index are higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 is the X-ray diffraction pattern of the seed crystal A1 obtained in Preparation Example 1-1 after calcination;
[0016] Figure 2 is the X-ray diffraction pattern of the seed crystal A1 obtained in Preparation Example 1-3 after calcination;
[0017] Figure 3 This is the SEM image of the ZSM-48 molecular sieve in Example 1. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] The first aspect of the present invention provides a hydroisomerization catalyst, which comprises a carrier and an active metal supported on the carrier, wherein the carrier comprises a ZSM-48 molecular sieve, wherein the molar ratio of silicon oxide to aluminum oxide in the ZSM-48 molecular sieve is not less than 40, and the specific surface area of the ZSM-48 molecular sieve is not less than 200 m 2 / g, the ZSM-48 molecular sieve has an ellipsoidal grain shape, a major diameter not exceeding 700nm and an aspect ratio of 1-3:1;
[0020] The active metal is selected from at least one of Pt, Pd, Ni and Co.
[0021] The hydroisomerization catalyst carrier of the present invention contains a ZSM-48 molecular sieve with a specific morphology. The ZSM-48 molecular sieve has an ellipsoidal morphology with a small aspect ratio, a high silicon-aluminum ratio, and a large specific surface area. When the hydroisomerization catalyst is used for the hydroisomerization of waxy oil, the product yield and viscosity index are higher.
[0022] According to a preferred embodiment of the present invention, the specific surface area of the ZSM-48 molecular sieve is 200-280m 2 / g.
[0023] Preferably, the aspect ratio of the ZSM-48 molecular sieve is 1-2:1.
[0024] According to a preferred embodiment of the present invention, the pore volume of the ZSM-48 molecular sieve is 0.20-0.30 ml / g.
[0025] According to a preferred embodiment of the present invention, the crystal size of the ZSM-48 molecular sieve is 300-700 nm, preferably 400-600 nm.
[0026] Under the above preferred conditions, the molecular sieve has better diffusion performance of isomerized products, thereby improving the catalytic effect of the hydroisomerization catalyst.
[0027] According to a preferred embodiment of the present invention, the method for preparing the ZSM-48 molecular sieve comprises the following steps:
[0028] (1) providing a mixture containing a silicon source, an alkali source, an aluminum source, a template, water, a molecular sieve mother liquor, and a seed crystal;
[0029] (2) subjecting the mixture to a crystallization reaction; the conditions of the crystallization reaction include: reacting at 20° C.-50° C. for 1-20 h, reacting at 50° C.-80° C. for 1-34 h, and then reacting at 80° C.-180° C. for 1-70 h;
[0030] (3) The mixture obtained by the crystallization reaction in step (2) is subjected to solid-liquid separation to obtain ZSM-48 molecular sieve and molecular sieve mother liquor, and the molecular sieve mother liquor is returned to step (1);
[0031] The method further comprises an optional step (4), which comprises: acidifying and precipitating the molecular sieve mother liquor, and then performing solid-liquid separation, and returning the obtained filtrate to step (1);
[0032] The mass percentage of the added seed crystals in step (1) is not less than 10% of the mass percentage of the silicon source, where the silicon source is calculated as SiO2.
[0033] According to the present invention, the ZSM-48 molecular sieve is prepared by recycling the molecular sieve mother liquor and introducing crystal seeds, which is conducive to the formation of small crystals. In the present invention, the progress and temperature of the crystallization reaction are strictly controlled through three stages of crystallization processes at different temperatures. Compared with the prior art, the crystallization reaction process is set at a low temperature, which helps to control the growth of crystals.
[0034] In the present invention, it is understood by those skilled in the art that the molecular sieve mother liquor can be obtained by arbitrarily selecting the above step (3) or steps (3) and (4). When the method provided by the present invention includes step (4), it is understood by those skilled in the art that the filtrate provides at least part of the molecular sieve mother liquor described in step (1).
[0035] Preferably, the preparation method further comprises step (4). Adopting the above preferred implementation mode is conducive to obtaining a ZSM-48 molecular sieve with small crystals and high specific surface area.
[0036] According to a preferred embodiment of the present invention, the conditions of the crystallization reaction in step (2) include: reacting at 20°C-50°C for 6-20h, reacting at 50°C-80°C for 12-34h, and then reacting at 80°C-180°C for 48-70h. Wherein, 20°C-50°C means 20°C≤t1<50°C, 50°C-80°C means 50°C≤t2≤80°C, and 80°C-180°C means 80°C<t3≤180°C. Under the above preferred embodiment, the formation of small-grained ZSM-48 is favorable.
[0037] According to a preferred embodiment of the present invention, in step (4), the acidification deposition comprises: adding acid to the molecular sieve mother liquor to adjust the pH value to 5-7, preferably 5-6.5.
[0038] Preferably, the acidification deposition time is 0.5-4h.
[0039] The molecular sieve mother liquor obtained by the above preferred embodiment has the characteristic of an appropriate amount of seed crystals, and is further recycled to step (1) to participate in the reaction, which is conducive to the formation of a molecular sieve with a high specific surface area.
[0040] In the present invention, there is no specific limitation on the type of the acid described in step (4), as long as the above-mentioned pH adjustment effect can be achieved. Preferably, the acid can be at least one of hydrochloric acid, nitric acid, ammonium nitrate and ammonium chloride.
[0041] In the present invention, the ratio of reactants in the preparation process of ZSM-48 molecular sieve has a certain influence on the final performance of the molecular sieve. According to a preferred embodiment of the present invention, specifically, the composition of each component in the mixture in step (1) calculated by molar amount satisfies the following relationship:
[0042] The composition of each component calculated by molar amount satisfies the following relationship:
[0043] R / SiO2=0.01-0.40, preferably 0.01-0.08;
[0044] M + / SiO2=0.01-0.40, preferably 0.1-0.2;
[0045] Al2O3 / SiO2=0-0.02, preferably 0.01-0.015;
[0046] H2O / SiO2=5-30, preferably 5-20;
[0047] Wherein, SiO2 refers to SiO2 in the silicon source, R represents the template, and M + Indicates alkaline source.
[0048] In the present invention, the amount of seed crystals used in the preparation process of the ZSM-48 molecular sieve in the hydroisomerization catalyst is relatively large. According to a preferred embodiment of the present invention, the mass percentage of the added seed crystals in step (1) accounts for 10-30% of the mass percentage of the silicon source, and more preferably 20-30%. In the above preferred case, it is conducive to the formation of more crystal nuclei, and the prepared molecular sieve has the characteristics of small grains.
[0049] According to the present invention, preferably, in the mixture of step (1), the amount of the molecular sieve mother liquor is less than the amount of water. Further preferably, the mass percentage of the molecular sieve mother liquor added in step (1) to the total mass percentage of the molecular sieve mother liquor and water in step (1) is not more than 50%, more preferably 10-30%. In the above preferred case, it is helpful to form a molecular sieve with small crystals and high specific surface area.
[0050] According to a preferred embodiment of the present invention, the water may be deionized water.
[0051] The silicon source, alkali source, aluminum source and template agent in step (1) of the present invention have a wide range of choices, and the above raw materials are conventionally selected in the art. The above raw materials should generally be mixed into a uniform colloid by corresponding means, for example, by stirring.
[0052] According to a preferred embodiment of the present invention, the silicon source is selected from at least one of white carbon black, fumed silica, silica sol, water glass and tetraethyl orthosilicate; more preferably, silica sol.
[0053] According to a preferred embodiment of the present invention, the alkali source is selected from alkaline metal salts, preferably at least one of calcium hydroxide, potassium hydroxide and sodium hydroxide; more preferably sodium hydroxide.
[0054] According to a preferred embodiment of the present invention, the aluminum source is selected from at least one of pseudo-boehmite, aluminum isopropoxide, aluminum sulfate and sodium aluminate; and pseudo-boehmite is further preferred.
[0055] According to a preferred embodiment of the present invention, the template is selected from at least one of ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-hexanediamine, hexamethylammonium hydroxide, hexamethylammonium chloride and hexamethylammonium bromide, and is further preferably at least one of 1,6-hexanediamine, hexamethylammonium bromide, hexamethylammonium chloride and hexamethylammonium hydroxide.
[0056] According to a preferred embodiment of the present invention, the seed crystal in the ZSM-48 molecular sieve preparation process is a ZSM-48 molecular sieve seed crystal, and the molar ratio of silicon oxide to aluminum oxide in the ZSM-48 molecular sieve seed crystal is not less than 40, preferably 45-500. The silicon-aluminum ratio in the ZSM-48 molecular sieve seed crystal mainly depends on the feeding and preparation method of the silicon source and aluminum source in the raw material.
[0057] In the XRD diffraction pattern of the ZSM-48 molecular sieve raw powder synthesized by the prior art method after calcination, the peak position of the diffraction peak is generally at 7.5°, 21.2°, 22.8°, and 31.3° at 2θ angles, wherein the diffraction peak at 21°-22° is the highest, while the diffraction peak intensity at 7°-8° is weaker. The researchers of the present invention have found that by adopting a specific synthesis method, the preferred ZSM-48 molecular sieve seed of the present invention can be prepared, and in the X-ray diffraction pattern after calcination, the relative peak height of the diffraction peak at 7°-8° at 2θ angle is significantly higher than the relative peak height of the diffraction peak at 7°-8° in the molecular sieve obtained by the prior art.
[0058] According to a preferred embodiment of the present invention, the peak height of the diffraction peak with a 2θ angle of 21°-22° is taken as the reference value, and the peak height of the diffraction peak with a 2θ angle of 7°-8° in the present invention is not less than 70% of the reference value, and further preferably, the peak height of the diffraction peak with a 2θ angle of 7°-8° is 70%-135% of the reference value; for example, the lower limit of the peak height range of the diffraction peak of 7°-8° can be 75%, 80%, 90% of the reference value, etc., and the upper limit of the peak height range of the diffraction peak of 7°-8° can be 135%, 120%, 110%, 100% of the reference value, etc. Due to the influence of factors such as samples and instruments, the specific peak position of the 2θ angle in the present invention may have a deviation of ±0.5°. The purpose of the calcination is to remove impurities such as templates in the molecular sieve raw powder to obtain more accurate XRD characterization results, and will not substantially affect the diffraction peaks in the XRD spectrum of the molecular sieve itself. Therefore, the calcination conditions are based on the removal of impurities. For example, it can be calcined at 400-700°C for 1-8h. The ZSM-48 molecular sieve seed crystals in the preparation example of the present invention were calcined at 600°C for 4h before XRD characterization.
[0059] According to a preferred embodiment of the present invention, the method for preparing the seed crystal includes contacting a reaction mixture under crystallization conditions, wherein the reaction mixture includes a silicon source, an alkali source, an aluminum source, a template and water. The selection range of the silicon source, alkali source, aluminum source and template can be the same as above, and will not be repeated here; the types of the selected silicon source, alkali source, aluminum source and template can be the same as or different from the types of the silicon source, alkali source, aluminum source and template described in the above molecular sieve preparation process. Preferably, in the seed crystal preparation process, the content of each component in the reaction mixture satisfies the following relationship:
[0060] R / SiO2=0.01-0.50, more preferably 0.01-0.3;
[0061] H2O / SiO2=5-50, more preferably 5-20;
[0062] M+ / SiO2=0.01-0.50, more preferably 0.01-0.15;
[0063] Al2O3 / SiO2=0-0.02; more preferably 0.01-0.017;
[0064] Wherein, R represents a template, and M+ represents an alkali source.
[0065] According to a preferred embodiment of the present invention, the preparation method of the seed mainly includes three steps of crystallization, and the temperature of each crystallization is higher than the previous crystallization temperature. Specifically, the first step crystallization temperature t1 satisfies 15℃≤t1<50℃, preferably carried out at room temperature, more preferably 20℃≤t1≤45℃, and the first step crystallization time is 5-24h, preferably 6-15h; the second step crystallization temperature t2 satisfies 50℃≤t2<100℃, preferably 60℃≤t2≤80℃, and the second step crystallization time is 0.5-36h, preferably 5-30h; the third step crystallization temperature t3 satisfies 100℃≤t3≤200℃, preferably 120℃≤t3≤190℃, and the third step crystallization time is 10-96h, preferably 20-80h.
[0066] According to a preferred embodiment of the present invention, the process of preparing the seed crystals further includes performing solid-liquid separation on the crystallization product to obtain the seed crystals.
[0067] The seed crystals obtained by the above preferred embodiment are used for the preparation of the above molecular sieve, which is conducive to obtaining small crystal products.
[0068] In order to obtain the ZSM-48 molecular sieve of the present invention, the reaction system after the above crystallization can be further subjected to solid-liquid separation and drying and other operations. The methods and conditions for solid-liquid separation and drying are conventional operations in the art and are not repeated here. For example, the reaction product can be filtered and then dried at 120° C. for 6 hours to obtain the molecular sieve.
[0069] According to a preferred embodiment of the present invention, in the hydroisomerization catalyst, the active metal content in terms of element is 0.1-2% by weight, preferably 0.2-0.6% by weight, based on the total amount of the catalyst.
[0070] According to a preferred embodiment of the present invention, the content of the molecular sieve on a dry basis is 20-80% by weight, preferably 40-70% by weight, based on the total amount of the catalyst.
[0071] According to a preferred embodiment of the present invention, the hydroisomerization catalyst further contains a binder. The type of the binder can be selected in a wide range, and preferably, the binder can be aluminum oxide and / or silicon oxide.
[0072] According to a preferred embodiment of the present invention, based on the total amount of the catalyst, the content of the binder is 20-80% by weight, preferably 30-70% by weight.
[0073] The hydroisomerization catalyst of the present invention has excellent catalytic effect, higher isomerization product yield and viscosity index, and lower pour point.
[0074] The second aspect of the present invention provides a method for preparing the hydroisomerization catalyst described in the first aspect, which comprises mixing the ZSM-38 molecular sieve with an optional binder and / or a binder precursor, and then optionally molding and drying to obtain a carrier, and then introducing an active metal into the carrier by an impregnation method.
[0075] The precursor of the binder may be a substance that is converted into the binder in a subsequent process, and the present invention has no particular limitation on this.
[0076] The “optionally forming” means that forming may be performed or not, and those skilled in the art may make a choice based on the specific application scenario of the catalyst.
[0077] In the present invention, the molding (for example, extrusion molding), drying and impregnation methods are all conventional technical means in the art, and the selection range of the binder and active metal is the same as mentioned above and will not be repeated here.
[0078] The third aspect of the present invention provides a method for hydroisomerization treatment of hydrocarbon oil, comprising: under hydroisomerization conditions, contacting a feedstock oil with a hydroisomerization catalyst, wherein the feedstock oil is selected from at least one of cracking tail oil, bio-jet fuel production feedstock, C5C6 isomerization feedstock, and Fischer-Tropsch synthesis wax, and the hydroisomerization catalyst is the hydroisomerization catalyst described in the first aspect.
[0079] Preferably, the conditions for the hydroisomerization include: a temperature of 200-500°C, preferably 250-400°C; a pressure of 1-30 MPa, preferably 2-20 MPa; a volume space velocity of 0.1-5 h -1 , preferably 0.1-3h -1 ; The volume ratio of hydrogen to oil is 50-3000, preferably 300-3000.
[0080] According to the hydrocarbon oil hydroisomerization treatment method of the present invention, by using the hydroisomerization catalyst provided by the present invention, the yield and viscosity index of the obtained product are higher, and a significant effect is achieved.
[0081] The present invention will be described in detail below through examples.
[0082] In the following examples and comparative examples, a Bruker D5005 diffractometer was used to perform XRD characterization on the samples, using Cu Kα rays (λ=0.154 nm), a tube voltage of 40 kV, a tube current of 30 mA, a scanning range of 5°-35°, a step of 0.013°, and 1 step per second. A Hitachi S-4800 scanning electron microscope (SEM) was used to characterize the sample morphology and size, with an accelerating voltage of 20 kV.
[0083] The composition of the samples was determined using a 3271E X-ray fluorescence spectrometer (XRF) produced by Rigaku Corporation. The sample preparation method was the tablet pressing method, and the measurement conditions were an end-window rhodium target, a tube voltage of 50 kV, and a tube current of 50 mA.
[0084] The dry basis of molecular sieve and pseudo-boehmite in the examples refers to the weight after calcination at 600° C. for 2 h.
[0085] The pore structure parameters of the product, such as specific surface area and pore volume, were measured by nitrogen adsorption and BET method.
[0086] The following preparation examples are used to illustrate the preparation of seed crystals.
[0087] Preparation Example 1-1
[0088] Aluminum sulfate, hexamethyldiamine hydroxide (HMOH), sodium hydroxide and deionized water were mixed in a certain proportion, stirred for 30 minutes and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMOH):n(Na + ):n(H2O):n(SiO2)=0.01:0.03:0.3:8:1, the mixture was transferred into a crystallization kettle and crystallized for 6 hours at room temperature with stirring at a speed of 400rpm; then crystallized at 80℃ for 24 hours, and then heated to 180℃ for crystallization for 48 hours. After the crystallization, the solid product was filtered and dried at 120℃ for 6 hours. The obtained product was seed A1. After the crystallization, the product was filtered and dried to obtain seed A1. After the seed A1 was calcined at 600℃ for 4 hours, the XRD diffraction peaks were seen. Figure 1 .
[0089] Preparation Example 1-2
[0090] Sodium aluminate, hexamethyldiamine chloride (HMCl), sodium hydroxide and deionized water were mixed in a certain proportion, stirred for 30 minutes and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.004:0.03:0.3:21:1, the mixture was transferred into a crystallization kettle, and crystallized for 12h under stirring at room temperature, with a stirring speed of 350rpm; crystallized for 12h at 60℃ and for 48h at 160℃. After the crystallization, the product was filtered and dried at 120℃ for 6h. The product obtained by filtering and drying after the crystallization was seed A2.
[0091] Preparation Example 1-3
[0092] Sodium aluminate, hexamethyldiamine chloride (HMCl), sodium hydroxide and deionized water were mixed in a certain proportion, stirred for 30 minutes and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.004:0.03:0.3:21:1, the mixture was transferred into a crystallization kettle, and crystallized for 12h under stirring at room temperature, with a stirring speed of 350rpm; crystallized for 60h at 170℃, and the product obtained by filtering and drying after the crystallization was seed A3. After calcining seed A3 at 600℃ for 4h, XRD showed Figure 2 .
[0093] The following examples are used to illustrate the preparation of hydroisomerization catalysts.
[0094] Example 1
[0095] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.01:0.03:0.3:10:1. The added mass percentage of the molecular sieve mother liquid accounts for 30% of the total mass percentage of the molecular sieve mother liquid and water in step (1), and 25% of the mass of SiO2 is added as ZSM-48 seed crystal A1;
[0096] (2) The mixture was transferred into a crystallization reactor, stirred at room temperature for 6 h, crystallized at 80 °C for 24 h, and crystallized at 170 °C for 48 h;
[0097] (3) After the crystallization is completed, the ZSM-48 molecular sieve and the molecular sieve mother liquor are obtained by filtering, and the molecular sieve mother liquor is returned to step (1);
[0098] After drying at 120°C for 6 hours, the product ZSM-48 molecular sieve was obtained and recorded as Z-1. The XRF analysis results of the silicon-aluminum ratio and the specific surface area of the prepared ZSM-48 molecular sieve are shown in Table 1, and the scanning electron microscope image is shown in Figure 3 Its morphology is ellipsoidal, the particle major diameter is 300-700nm, and the ratio of major diameter to minor diameter is about 1.1-1.4:1.
[0099] 100 g of Z-1 molecular sieve was mixed with 100 g of alumina, extruded and dried to obtain a carrier.
[0100] Pour 1 gram of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then it is calcined under the condition of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named IC-1.
[0101] Example 2
[0102] (1) Sodium aluminate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.004:0.03:0.3:20:1, the mass percentage of the added molecular sieve mother liquor to the total mass percentage of the molecular sieve mother liquor and water in step (1) is 20%, and 15% of the mass of SiO2 ZSM-48 seed crystals A2 are added;
[0103] (2) transferring the above mixture into a crystallization kettle, crystallizing at 40°C for 12 h, at 80°C for 10 h, and at 170°C for 48 h;
[0104] (3) After the crystallization is completed, the ZSM-48 molecular sieve and the molecular sieve mother liquor are obtained by filtering, and the molecular sieve mother liquor is returned to step (1);
[0105] The product ZSM-48 molecular sieve was obtained by drying at 120°C for 6 hours and was recorded as Z-2. The XRF analysis results and specific surface area data of the prepared ZSM-48 molecular sieve are shown in Table 1. Its morphology is ellipsoidal, the particle major diameter is 300-600nm, and the ratio of major diameter to minor diameter is about 1.1-1.4:1.
[0106] 100 g of Z-2 molecular sieve was mixed with 40 g of alumina, extruded and dried to obtain a carrier.
[0107] Pour 1 gram of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then it is calcined under the state of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named IC-2.
[0108] Example 3
[0109] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing an acidified molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.018:0.03:0.3:30:1, the mass percentage of the added molecular sieve mother liquor to the total mass percentage of the molecular sieve mother liquor and water in step (1) is 30%, and 25% of the mass of SiO2 ZSM-48 seed crystals A1 are added;
[0110] (2) The mixture was transferred into a crystallization reactor, stirred at room temperature for 6 h, crystallized at 80 °C for 24 h, and crystallized at 170 °C for 48 h;
[0111] (3) After the crystallization is completed, the ZSM-48 molecular sieve and the molecular sieve mother liquor are filtered to obtain, and the molecular sieve mother liquor is acidified and precipitated. The acidification process is to adjust the pH value of the mother liquor to 6.2 with ammonium chloride, stand for 2 hours, and return the filtrate obtained by filtration to step (1);
[0112] The product ZSM-48 molecular sieve was obtained by drying at 120°C for 6 hours and was recorded as Z-3. The XRF analysis results and specific surface area data of the obtained ZSM-48 molecular sieve are shown in Table 1. Its morphology is ellipsoidal, the particle major diameter is 300-600nm, and the ratio of major diameter to minor diameter is about 1.1-1.5:1.
[0113] 100 g of Z-3 molecular sieve was mixed with 40 g of alumina, extruded and dried to obtain a carrier.
[0114] Pour 1 gram of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then, it is calcined under the state of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named IC-3.
[0115] Example 4
[0116] (1) Sodium aluminate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na +):n(H2O):n(SiO2)=0.018:0.03:0.3:20:1, the mass percentage of the added molecular sieve mother liquor to the total mass percentage of the molecular sieve mother liquor and water in step (1) is 20%, and 15% of the mass of SiO2 ZSM-48 seed crystals A2 are added;
[0117] (2) transferring the above mixture into a crystallization kettle and crystallizing at 40°C for 12 h, at 80°C for 6 h, and at 170°C for 48 h;
[0118] (3) After the crystallization is completed, the ZSM-48 molecular sieve and the molecular sieve mother liquor are filtered to obtain, and the molecular sieve mother liquor is acidified and precipitated. The acidification process is to adjust the pH value of the mother liquor to 5.6 with ammonium chloride, stand for 3 hours, and return the filtrate obtained by filtration to step (1);
[0119] The product ZSM-48 molecular sieve was obtained by drying at 120°C for 6 hours and was recorded as Z-4. The XRF analysis results and specific surface area data of the obtained ZSM-48 molecular sieve are shown in Table 1. Its morphology is ellipsoidal, the particle major diameter is 400-700nm, and the ratio of major diameter to minor diameter is about 1.1-1.4:1.
[0120] 100 g of Z-4 molecular sieve was mixed with 40 g of alumina, extruded and dried to obtain a carrier.
[0121] Pour 0.63 g of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 g of deionized water and stir until uniform. Pour 100 g of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then, it is calcined under the condition of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named IC-4.
[0122] Example 5
[0123] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.0125:0.03:0.3:30:1. The mass percentage of the added molecular sieve mother liquid to the total mass percentage of the molecular sieve mother liquid and water in step (1) is 15%, and 15% of the mass of SiO2 ZSM-48 seed crystal A1 is added;
[0124] (2) The mixture was transferred into a crystallization reactor, stirred at room temperature for 6 h, crystallized at 80 °C for 24 h, and crystallized at 170 °C for 48 h;
[0125] (3) After the crystallization is completed, the ZSM-48 molecular sieve and the molecular sieve mother liquor are obtained by filtering, and the molecular sieve mother liquor is returned to step (1);
[0126] The product ZSM-48 molecular sieve was obtained by drying at 120°C for 6 hours and was recorded as Z-5. The XRF analysis results of the silicon-aluminum ratio and the specific surface area of the prepared ZSM-48 molecular sieve are shown in Table 1. Its morphology is ellipsoidal, the particle major diameter is 300-700nm, and the ratio of major diameter to minor diameter is about 1.1-1.4:1.
[0127] 100 g of Z-5 molecular sieve was mixed with 100 g of alumina, extruded and dried to obtain a carrier.
[0128] Pour 0.63 g of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 g of deionized water and stir until uniform. Pour 100 g of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor was dried at 120°C for 4 hours. Then it was calcined under the condition of air flow, the calcination temperature was 450°C, and the time was 4 hours. The semi-finished catalyst was placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst was named IC-5.
[0129] Example 6
[0130] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.0125:0.03:0.3:30:1. The added mass percentage of the molecular sieve mother liquid accounts for 20% of the total mass percentage of the molecular sieve mother liquid and water in step (1), and 20% of the mass of SiO2 in ZSM-48 seed crystal A1 is added;
[0131] (2) The mixture was transferred into a crystallization reactor, stirred at room temperature for 6 h, crystallized at 80 °C for 24 h, and crystallized at 170 °C for 48 h;
[0132] (3) After the crystallization is completed, the ZSM-48 molecular sieve and the molecular sieve mother liquor are obtained by filtering, and the molecular sieve mother liquor is returned to step (1);
[0133] The product ZSM-48 molecular sieve was obtained by drying at 120°C for 6 hours and was recorded as Z-6. The XRF analysis results of the silicon-aluminum ratio and the specific surface area of the prepared ZSM-48 molecular sieve are shown in Table 1. Its morphology is ellipsoidal, the particle major diameter is 300-700nm, and the ratio of major diameter to minor diameter is about 1.1-1.4:1.
[0134] 100 g of Z-6 molecular sieve was mixed with 100 g of alumina, extruded and dried to obtain a carrier.
[0135] Pour 1 gram of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then it is calcined under the state of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named IC-6.
[0136] Example 7
[0137] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.0125:0.02:0.2:20:1. The added mass percentage of the molecular sieve mother liquid accounts for 20% of the total mass percentage of the molecular sieve mother liquid and water in step (1), and 20% of the mass of SiO2 in ZSM-48 seed crystal A1 is added;
[0138] (2) The mixture was transferred into a crystallization reactor, stirred at room temperature for 6 h, crystallized at 80 °C for 24 h, and crystallized at 170 °C for 48 h;
[0139] (3) After the crystallization is completed, the ZSM-48 molecular sieve and the molecular sieve mother liquor are obtained by filtering, and the molecular sieve mother liquor is returned to step (1);
[0140] The product ZSM-48 molecular sieve was obtained by drying at 120°C for 6 hours and was recorded as Z-7. The XRF analysis results of the silicon-aluminum ratio and the specific surface area of the prepared ZSM-48 molecular sieve are shown in Table 1. Its morphology is ellipsoidal, the particle major diameter is 300-700nm, and the ratio of major diameter to minor diameter is about 1.1-1.4:1.
[0141] 100 g of Z-7 molecular sieve was mixed with 100 g of alumina, extruded and dried to obtain a carrier.
[0142] Pour 1.1 g of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 g of deionized water and stir until uniform. Pour 100 g of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor was dried at 120°C for 4 hours. Then it was calcined under the condition of air flow, the calcination temperature was 450°C, and the time was 4 hours. The semi-finished catalyst was placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst was named IC-7.
[0143] Example 8
[0144] The method in Example 1 was followed, except that the amount of Z-1 molecular sieve was 50 g. The obtained catalyst was named IC-8.
[0145] Example 9
[0146] The method in Example 1 was followed, except that the amount of tetraammine dichloroplatinum was 0.5 g. The obtained catalyst was named IC-9.
[0147] Comparative Example 1
[0148] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.0125:0.03:0.3:30:1. Add 25% of the mass of SiO2 in ZSM-48 seed crystal A3. The mass percentage of the added molecular sieve mother liquid to the total mass percentage of the molecular sieve mother liquid and water in step (1) is 20%;
[0149] (2) The mixture was transferred into a crystallization reactor, stirred at room temperature for 6 h, crystallized at 80 °C for 24 h, and crystallized at 170 °C for 48 h;
[0150] (3) After the crystallization is completed, the ZSM-48 molecular sieve DZ-1 is obtained by filtering and drying. The XRF analysis results and specific surface area data of the obtained ZSM-48 molecular sieve are shown in Table 1. Its morphology is rod-shaped, and the ratio of the length to the short diameter is about 7:1.
[0151] 100 g of DZ-1 molecular sieve was mixed with 100 g of alumina, extruded and dried to obtain a carrier.
[0152] Pour 1 gram of dichlorotetraamineplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then, it is calcined under the state of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named DIC-1.
[0153] Comparative Example 2
[0154] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide and deionized water were mixed in a certain proportion, stirred for 30 minutes and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.004.03:0.3:30:1. Add 25% of the mass of SiO2 ZSM-48 seed crystal A3;
[0155] (2) The mixture was transferred into a crystallization reactor, stirred at room temperature for 6 h, crystallized at 80 °C for 24 h, and crystallized at 170 °C for 48 h;
[0156] (3) After the crystallization is completed, the ZSM-48 molecular sieve DZ-2 is obtained by filtering and drying. The XRF analysis results and specific surface area data of the obtained ZSM-48 molecular sieve are shown in Table 1. Its morphology is rod-shaped, and the ratio of the length to the short diameter is about 5:1.
[0157] 100 g of DZ-2 molecular sieve was mixed with 40 g of alumina, extruded and dried to obtain a carrier.
[0158] Pour 1 gram of tetraammine dichloroplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then, it is calcined under the state of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named DIC-2.
[0159] Comparative Example 3
[0160] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na +):n(H2O):n(SiO2)=0.018:0.03:0.3:30:1. Add 25% of the mass of SiO2 in ZSM-48 seed crystal A1. The mass percentage of the added molecular sieve mother liquid to the total mass percentage of the molecular sieve mother liquid and water in step (1) is 20%;
[0161] (2) transferring the above mixture into a crystallization kettle and crystallizing at 170° C. for 48 h;
[0162] (3) After the crystallization is completed, the ZSM-48 molecular sieve DZ-3 is obtained by filtering and drying. The XRF analysis results and specific surface area data of the obtained ZSM-48 molecular sieve are shown in Table 1. Its morphology is rod-shaped, and the ratio of the length to the short diameter is about 6:1.
[0163] 100 g of DZ-3 molecular sieve was mixed with 40 g of alumina, extruded and dried to obtain a carrier.
[0164] Pour 1 gram of dichlorotetraamineplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then, it is calcined under the state of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named DIC-3.
[0165] Comparative Example 4
[0166] (1) Aluminum sulfate, hexamethyldiamine chloride (HMCl), sodium hydroxide, and deionized water containing molecular sieve mother liquor were mixed in a certain proportion, stirred for 30 minutes, and then silica sol was added. The molar ratio of each substance was n(Al2O3):(HMCl):n(Na + ):n(H2O):n(SiO2)=0.018:0.03:0.3:30:1. Add 5% of the mass of SiO2 in ZSM-48 seed crystal A1. The mass percentage of the added molecular sieve mother liquid to the total mass percentage of the molecular sieve mother liquid and water in step (1) is 20%;
[0167] (2) transferring the above mixture into a crystallization kettle and crystallizing at 170° C. for 48 h;
[0168] (3) After the crystallization is completed, the ZSM-48 molecular sieve DZ-4 is obtained by filtering and drying. The XRF analysis results and specific surface area data of the obtained ZSM-48 molecular sieve are shown in Table 1. Its morphology is rod-shaped, and the ratio of length to short diameter is about 7:1.
[0169] 100 g of DZ-4 molecular sieve was mixed with 40 g of alumina, extruded and dried to obtain a carrier.
[0170] Pour 1 gram of dichlorotetraamineplatinum (containing 57.3% Pt by mass) into 100 grams of deionized water and stir until uniform. Pour 100 grams of the carrier into the above solution and soak at room temperature for 4 hours. Subsequently, the above catalyst precursor is dried at 120°C for 4 hours. Then it is calcined under the state of passing air flow, the calcination temperature is 450°C, and the time is 4 hours. The semi-finished catalyst is placed in a hydrogen atmosphere again and reduced at 400°C for 4 hours to obtain a catalyst. The obtained catalyst is named DIC-4.
[0171] IC-1 to IC-9 and DIC-1 to DIC-4 were evaluated using the following evaluation method:
[0172] 50g of catalyst was loaded into a high-pressure hydrogenation reactor. Hydrocracking tail oil was injected into the reactor from top to bottom for reaction. The reaction conditions were shown in Table 2 below, and the analysis data of the hydrocracking tail oil were shown in Table 3. After the reaction, the product was distilled to remove light components less than 370 degrees, and the components greater than 370 degrees were analyzed and the yield was calculated. The results are shown in Table 4.
[0173] Table 1
[0174]
[0175] Table 2 Catalyst evaluation conditions
[0176] Reaction conditions Numeric Pressure, MPa 15 <![CDATA[Air speed, h -1 > 1.2 Reaction temperature, °C 335 Hydrogen to oil ratio, v / v 400
[0177] Table 3 Hydrocracking tail oil analysis results
[0178] Analyze Project Analyze the data Analytical methods <![CDATA[Density at 20℃ / (kg / m 3 )]]> 842.8 SH / T0604-2000 <![CDATA[Kinematic viscosity / (mm 2 / s)]]> 40℃ 20.138 GB / T 265-88 100℃ 4.552 GB / T 265-88 Pour point / ℃ +36 SH / T 0771-2005 Nitrogen mass fraction / (μg / g) <1 NB / SH / T 0704-2010 Sulfur mass fraction / (μg / g) 5 SH / T 0842-2010
[0179] Table 4 Evaluation results
[0180]
[0181] It can be seen from the results of the above examples that when the hydroisomerization catalyst of the present invention is applied to hydrocracking tail oil isomerization dewaxing, the product yield and viscosity index are higher.
[0182] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydroisomerization catalyst, comprising a carrier and an active metal supported on the carrier, wherein the carrier comprises a ZSM-48 molecular sieve, wherein the molar ratio of silicon oxide to aluminum oxide in the ZSM-48 molecular sieve is not less than 40, and the specific surface area of the ZSM-48 molecular sieve is not less than 200 m 2 / g, the ZSM-48 molecular sieve has an ellipsoidal grain shape, a major diameter not exceeding 700nm and an aspect ratio of 1-3:1; The active metal is selected from at least one of Pt, Pd, Ni and Co; The specific surface area of the ZSM-48 molecular sieve is 200-280m 2 / g; the aspect ratio of the ZSM-48 molecular sieve is 1-2:1; the grain size of the ZSM-48 molecular sieve is 300-700nm; The preparation method of the ZSM-48 molecular sieve comprises the following steps: (1) Providing a mixture containing a silicon source, an alkali source, an aluminum source, a template, water, a molecular sieve mother liquor and a seed crystal; (2) subjecting the mixture to a crystallization reaction; the conditions of the crystallization reaction include: reacting at 20°C-50°C for 1-20 hours, reacting at 50°C-80°C for 1-34 hours, and then reacting at 80°C-180°C for 1-70 hours; (3) The mixture obtained by the crystallization reaction in step (2) is subjected to solid-liquid separation to obtain ZSM-48 molecular sieve and molecular sieve mother liquor, and the molecular sieve mother liquor is returned to step (1); The method further comprises an optional step (4), which comprises: acidifying and precipitating the molecular sieve mother liquor, and then performing solid-liquid separation, and returning the obtained filtrate to step (1); The mass percentage of the added seed crystals in step (1) is not less than 10% of the mass percentage of the silicon source, where the silicon source is calculated as SiO2; The method for preparing the seed crystal comprises contacting a reaction mixture under crystallization conditions, wherein the reaction mixture comprises a silicon source, an alkali source, an aluminum source, a template and water, and the crystallization conditions comprise: crystallizing at a temperature t1 for 5-24 hours, crystallizing at a temperature t2 for 0.5-36 hours, and crystallizing at a temperature t3 for 10-96 hours, 15°C≤t1<50°C, 50°C≤t2<100°C, and 100°C≤t3≤200°C.
2. The hydroisomerization catalyst according to claim 1, wherein The pore volume of the ZSM-48 molecular sieve is 0.20-0.30 ml / g.
3. The hydroisomerization catalyst according to claim 1 or 2, wherein The crystal size of the ZSM-48 molecular sieve is 400-600 nm.
4. The hydroisomerization catalyst according to claim 1, wherein The conditions of the crystallization reaction in step (2) include: reacting at 20°C-50°C for 6-20h, reacting at 50°C-80°C for 12-34h, and then reacting at 80°C-180°C for 48-70h.
5. The hydroisomerization catalyst according to claim 4, wherein In step (4), the acidification deposition comprises: adding acid to the molecular sieve mother liquor and adjusting the pH value to 5-7; the time of the acidification deposition is 0.5-4h.
6. The hydroisomerization catalyst according to claim 1, wherein The composition of each component in the mixture in step (1) calculated by molar amount satisfies the following relationship: R / SiO2=0.01-0.40; M + / SiO2=0.01-0.40; Al2O3 / SiO2=0-0.02; H2O / SiO2=5-30; Wherein, SiO2 refers to SiO2 in the silicon source, R represents the template, and M + Indicates alkaline source.
7. The hydroisomerization catalyst according to claim 6, wherein The composition of each component in the mixture in step (1) calculated by molar amount satisfies the following relationship: R / SiO2=0.01-0.08; M + / SiO2=0.1-0.2; Al2O3 / SiO2=0.01-0.015; H2O / SiO2=5-20.
8. The hydroisomerization catalyst according to claim 1, wherein The mass percentage of the added seed crystals in step (1) is 10-30% of the mass percentage of the silicon source; The mass percentage of the added molecular sieve mother liquor in step (1) to the total mass percentage of the molecular sieve mother liquor and water in step (1) is no more than 50%.
9. The hydroisomerization catalyst according to claim 8, wherein The mass percentage of the added molecular sieve mother liquor in step (1) to the total mass percentage of the molecular sieve mother liquor and water in step (1) is 10-30%.
10. The hydroisomerization catalyst according to claim 1, wherein The silicon source is selected from at least one of white carbon black, fumed silica, silica sol, water glass and tetraethyl orthosilicate; And / or, the alkali source is selected from alkaline metal salts; And / or, the aluminum source is selected from at least one of pseudo-boehmite, aluminum isopropoxide, aluminum sulfate and sodium aluminate; And / or, the template agent is selected from at least one of ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-hexanediamine, hexamethylammonium hydroxide, hexamethylammonium chloride and hexamethylammonium bromide.
11. The hydroisomerization catalyst according to claim 10, wherein The alkali source is at least one of calcium hydroxide, potassium hydroxide and sodium hydroxide.
12. The hydroisomerization catalyst according to claim 1, wherein The seed crystals are ZSM-48 molecular sieve seed crystals, the molar ratio of silicon oxide to aluminum oxide in the ZSM-48 molecular sieve seed crystals is not less than 40, and in the X-ray diffraction pattern of the ZSM-48 molecular sieve seed crystals after calcination, the peak height of the diffraction peak with a 2θ angle of 21°-22° is used as the reference value, and the peak height of the diffraction peak with a 2θ angle of 7°-8° is not less than 70% of the reference value.
13. The hydroisomerization catalyst according to claim 12, wherein The molar ratio of silicon oxide to aluminum oxide in the ZSM-48 molecular sieve seed crystal is 45-500. In the X-ray diffraction pattern of the ZSM-48 molecular sieve seed crystal after calcination, the peak height of the diffraction peak with a 2θ angle of 21°-22° is taken as the reference value, and the peak height of the diffraction peak with a 2θ angle of 7°-8° is 75%-135% of the reference value.
14. The hydroisomerization catalyst according to any one of claims 1 to 13, wherein Based on the total amount of the catalyst, the active metal content is 0.1-2% by weight in terms of element, and the molecular sieve content is 20-80% by weight in terms of dry basis; the catalyst also contains a binder.
15. The hydroisomerization catalyst according to claim 14, wherein Based on the total amount of catalyst, the active metal content is 0.2-0.6% by weight as an element, and the molecular sieve content is 40-70% by weight as a dry basis; The binder is aluminum oxide and / or silicon oxide; based on the total amount of the catalyst, the content of the binder is 20-80% by weight.
16. A method for hydroisomerization of hydrocarbon oil, comprising: Under hydroisomerization conditions, the feedstock oil is contacted with a hydroisomerization catalyst, wherein the feedstock oil is selected from at least one of cracking tail oil, bio-jet fuel production feedstock, C5C6 isomerization feedstock, and Fischer-Tropsch wax, and the hydroisomerization catalyst is the hydroisomerization catalyst according to any one of claims 1 to 15; The conditions of the hydroisomerization include: temperature of 200-500°C; pressure of 1-30MPa; volume space velocity of 0.1-5h -1 ; The volume ratio of hydrogen to oil is 50-3000.
17. The processing method according to claim 16, wherein: The conditions of the hydroisomerization include: temperature of 250-400°C; pressure of 2-20 MPa; volume space velocity of 0.1-3 h -1 ; The volume ratio of hydrogen to oil is 300-3000.