Silicon-based negative electrode material and preparation method thereof, battery and terminal

By combining a low silicon-oxygen-based silicon-based matrix and a high silicon-based silicon-based particle in the silicon-based negative electrode material, and setting a conductive layer and a carbon cladding layer on the surface, the problem of low cycling performance caused by volume expansion of the silicon-based material is solved. A silicon-based negative electrode material with high capacity and high cycle stability is achieved, improving the lithium embedded performance and structural stability of the battery.

CN116053452BActive Publication Date: 2024-11-15HUAWEI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310015238.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-31
Publication Date
2024-11-15
Estimated Expiration
2039-12-31

AI Technical Summary

Technical Problem

The volume of the silicon-based negative electrode material expands during charging and discharging, resulting in low battery circulation performance and cannot effectively replace traditional graphite negative electrode materials.

Method used

Using a combination material of a low silicon-oxygen-based silicon-based matrix and a high silicon-based particle, a conductive layer and an ion-conducting layer are arranged on the surface of the high silicon-based particle, and carbon is formed on the surface of the low silicon-based matrix. The cladding layer disperses high silicon-oxygen ratio silicon-based particles in the low silicon-oxygen ratio silicon-based matrix, controls the silicon-oxygen ratio and particle size distribution to alleviate volume expansion and improve structural stability.

Benefits of technology

The silicon-based anode material with high capacity and high cycle stability is achieved, reducing the volume change of the battery during lithium embedding, extending the cycle life, and improving the conductivity and expansion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116053452B_ABST
    Figure CN116053452B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention provides a silicon-based negative electrode material, including a low silicon-oxygen ratio silicon-based matrix, and high silicon-oxygen ratio silicon-based particles dispersed in the low silicon-oxygen ratio silicon-based matrix, the silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based matrix is ​​1:1, wherein 1<1≤2, the silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles is 1:1, wherein 0≤1≤1, the low silicon-oxygen ratio silicon-based matrix is ​​silicon dioxide, or the low silicon-oxygen ratio silicon-based matrix includes silicon dioxide and silicon-containing crystal particles dispersed in the silicon dioxide, the high silicon-oxygen ratio silicon-based particles are silicon particles, or the high silicon-oxygen ratio silicon-based particles include silicon dioxide and silicon-containing crystal particles dispersed in the silicon dioxide. The silicon-based negative electrode material has both high capacity and low expansion performance. The embodiment of the present invention also provides a preparation method of the silicon-based negative electrode material, and a battery and a terminal containing the silicon-based negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The application number of the original application is 201911425863.2, and the original application date is December 31, 2019. The entire contents of the original application are incorporated into this application by reference. Technical Field

[0002] The embodiments of the present invention relate to the technical field of lithium-ion batteries, and in particular to silicon-based negative electrode materials and preparation methods thereof, batteries and terminals. Background Art

[0003] Silicon has a theoretical specific capacity of 4200mAh / g and is one of the most studied negative electrode materials that is expected to replace commercial graphite. However, silicon will produce huge volume expansion and contraction during the charging and discharging process, which will cause the electrode structure to be destroyed and the battery capacity to decay rapidly. Compared with pure silicon materials, the volume expansion of silicon oxide materials is greatly reduced, but it is still very high compared with traditional graphite negative electrodes. Therefore, it is necessary to develop a low-expansion silicon-based negative electrode material to improve the cycle stability of the negative electrode. Summary of the invention

[0004] In view of this, an embodiment of the present invention provides a silicon-based negative electrode material having both higher capacity and lower expansion performance, so as to solve to a certain extent the problem of low battery cycle performance caused by excessive expansion effect of existing silicon-based materials.

[0005] Specifically, a first aspect of an embodiment of the present invention provides a silicon-based negative electrode material, comprising a low silicon-oxygen ratio silicon-based matrix, and high silicon-oxygen ratio silicon-based particles dispersed in the low silicon-oxygen ratio silicon-based matrix, the silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based matrix is ​​1:1, wherein 1<1≤2, the silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles is 1:1, wherein 0≤1≤1, the low silicon-oxygen ratio silicon-based matrix is ​​silicon dioxide, or the low silicon-oxygen ratio silicon-based matrix includes silicon dioxide and silicon-containing crystal particles dispersed in the silicon dioxide, the high silicon-oxygen ratio silicon-based particles are silicon particles, or the high silicon-oxygen ratio silicon-based particles include silicon dioxide and silicon-containing crystal particles dispersed in the silicon dioxide.

[0006] In an embodiment of the present invention, the low silicon-oxygen ratio silicon-based matrix is ​​grown in situ on the surface of the high silicon-oxygen ratio silicon-based particles.

[0007] In an embodiment of the present invention, the silicon-containing crystal particles are crystalline silicon and / or lithium-containing silicates.

[0008] In an embodiment of the present invention, the particle size of the high silicon-oxygen ratio silicon-based particles is 20nm-1000nm.

[0009] In an embodiment of the present invention, the particle size of the silicon-containing crystal particles is 2nm-15nm.

[0010] In an embodiment of the present invention, a conductive layer and / or an ion conductive layer is provided on the surface of the high silicon-oxygen ratio silicon-based particles.

[0011] In an embodiment of the present invention, the material of the conductive layer is selected from one or more of conductive polymers, carbonaceous materials, metals or alloys.

[0012] In the embodiment of the present invention, the material of the ion-conducting layer is selected from LiPO4, LiLaTiO4, Li7La3Zr2O 12 , LiAlO2, LiAlF4, LiAlS, Li2MgTiO4, Li6La3Zr 1.5 W 0.5 O 12 One or more of .

[0013] In an embodiment of the present invention, the thickness of the conductive layer is 2nm-150nm, and the thickness of the ion conductive layer is 2nm-150nm.

[0014] In an embodiment of the present invention, the silicon-based negative electrode material further includes a carbon coating layer coated on the surface of the low silicon-oxygen ratio silicon-based substrate.

[0015] In an embodiment of the present invention, the particle size of the silicon-based negative electrode material is 3 μm-8 μm.

[0016] The silicon-based negative electrode material provided in the first aspect of an embodiment of the present invention disperses high silicon-oxygen ratio silicon-based particles in a low silicon-oxygen ratio silicon-based matrix to achieve confined distribution of different silicon-oxygen concentrations, wherein the high silicon-oxygen ratio silicon-based particles can ensure that the negative electrode material has a high lithium insertion capacity, while the low silicon-oxygen ratio silicon-based matrix with a relatively small expansion effect can prevent the negative electrode material from undergoing a large volume change during the lithium insertion process, and the distribution around the high silicon-oxygen ratio silicon-based particles can effectively alleviate the volume expansion caused by the high silicon-oxygen ratio silicon-based particles, thereby inhibiting the breakage and pulverization of the silicon-based material and improving the cycle life of the silicon-based negative electrode material.

[0017] A second aspect of an embodiment of the present invention provides a method for preparing a silicon-based negative electrode material, comprising:

[0018] Silicon powder and silicon dioxide powder are mixed at a silicon-oxygen ratio of 1:11, wherein 0<11≤1, and then calcined and ground to obtain silicon-based particles with a high silicon-oxygen ratio; or silicon particles are directly used as silicon-based particles with a high silicon-oxygen ratio;

[0019] Silicon powder and silicon dioxide powder are mixed at a silicon-oxygen ratio of 1:11, wherein 1<11<2, and then calcined under vacuum or protective atmosphere to form vapor with a low silicon-oxygen ratio; or silicon dioxide powder alone is calcined under vacuum or protective atmosphere to form vapor with a low silicon-oxygen ratio;

[0020] The vapor of the low silicon-oxygen ratio is deposited on the high silicon-oxygen ratio silicon-based particles to form a low silicon-oxygen ratio silicon-based matrix to obtain a silicon-based negative electrode material, wherein the silicon-based negative electrode material includes a low silicon-oxygen ratio silicon-based matrix and high silicon-oxygen ratio silicon-based particles dispersed in the low silicon-oxygen ratio silicon-based matrix, the silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based matrix is ​​1:1, wherein 1<1≤2, the silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles is 1:1, wherein 0≤1≤1, the low silicon-oxygen ratio silicon-based matrix is ​​silicon dioxide, or the low silicon-oxygen ratio silicon-based matrix includes silicon dioxide and silicon-containing crystal particles dispersed in the silicon dioxide, the high silicon-oxygen ratio silicon-based particles are silicon particles, or the high silicon-oxygen ratio silicon-based particles include silicon dioxide and silicon-containing crystal particles dispersed in the silicon dioxide.

[0021] In an embodiment of the present invention, the preparation method further comprises:

[0022] A conductive layer and / or an ion-conducting layer is prepared on the surface of the high silicon-oxygen ratio silicon-based particles by a sol-gel method or a vapor deposition method.

[0023] In an embodiment of the present invention, in the step of calcining and grinding to prepare silicon-based particles with a high silicon-oxygen ratio, the calcination is carried out under vacuum or protective atmosphere at a calcination temperature of 1100°C-1600°C.

[0024] In the embodiment of the present invention, the calcination temperature for forming the vapor with low silicon-oxygen ratio by calcination under vacuum or protective atmosphere is 800° C.-1400° C., and the calcination time is 2-40 hours.

[0025] In an embodiment of the present invention, when the silicon-containing crystal particles in the high silicon-oxygen ratio silicon-based particles include lithium-containing silicates, the preparation method further comprises introducing a lithium source during the preparation of the high silicon-oxygen ratio silicon-based particles.

[0026] In an embodiment of the present invention, when the silicon-containing crystal particles in the low silicon-oxygen ratio silicon-based matrix include lithium-containing silicates, the preparation method further comprises introducing a lithium source during the process of forming the low silicon-oxygen ratio vapor.

[0027] In an embodiment of the present invention, the preparation method further comprises: forming a carbon coating layer on the surface of the low silicon-oxygen ratio silicon-based substrate.

[0028] The preparation method provided in the second aspect of the embodiment of the present invention has a simple process and can obtain silicon-based negative electrode materials with different silicon-oxygen concentration confined distributions, so that the silicon-based negative electrode materials have both high capacity and high cycle stability.

[0029] A third aspect of an embodiment of the present invention provides a battery, comprising a positive electrode plate, a negative electrode plate, a separator, and an electrolyte, wherein the negative electrode plate comprises a negative electrode active material, and the negative electrode active material comprises the silicon-based negative electrode material described in the first aspect of the present invention.

[0030] The battery provided by the embodiment of the present invention has high capacity and better cycle performance.

[0031] An embodiment of the present invention also provides a terminal, including a terminal shell, and a circuit board and a battery located inside the terminal shell, wherein the battery is electrically connected to the circuit board for powering the circuit board, and the battery includes the battery described in the third aspect of the embodiment of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram of the structure of a lithium-ion secondary battery provided by an embodiment of the present invention;

[0033] Figure 2 A schematic diagram of the structure of a silicon-based negative electrode material provided in an embodiment of the present invention;

[0034] Figure 3 Schematic diagram of the structure of silicon-based particles with a high silicon-oxygen ratio in an embodiment of the present invention;

[0035] Figure 4 A schematic diagram of the structure of a terminal provided by an embodiment of the present invention;

[0036] Figure 5 A SEM (Scanning Electron Microscope) image of a silicon-based negative electrode material provided in an embodiment of the present invention;

[0037] Figure 6A-6C This is a cross-sectional SEM (Scanning Electron Microscope) image of the silicon-based negative electrode material provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0038] The embodiments of the present invention will be described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0039] The embodiment of the present invention provides a silicon-based negative electrode material, which can be used to make a negative electrode of a lithium-ion secondary battery. Figure 1As shown, the core components of a lithium-ion secondary battery include a positive electrode material 101, a negative electrode material 102, an electrolyte 103, a diaphragm 104, and corresponding connecting accessories and circuits. Among them, the positive electrode material 101 and the negative electrode material 102 can deintercalate lithium ions to achieve energy storage and release, the electrolyte is a carrier for the transmission of lithium ions between the positive and negative electrodes, and the diaphragm 104 can pass lithium ions but is not conductive, thereby separating the positive and negative electrodes to prevent short circuits. Among them, the positive and negative electrode materials are the main parts that play the energy storage function, and are the most direct embodiment of the energy density, cycle performance and safety performance of the battery cell. Silicon-based negative electrode materials have attracted attention in the industry due to their high gram capacity. However, silicon-based negative electrode materials have large volume expansion and high surface activity, resulting in poor battery cycle performance. To solve this problem, an embodiment of the present invention provides a silicon-based negative electrode material that has high capacity and high structural stability.

[0040] like Figure 2 As shown, the silicon-based negative electrode material 10 provided by the embodiment of the present invention comprises a low silicon-oxygen ratio silicon-based matrix 1, and high silicon-oxygen ratio silicon-based particles 2 dispersed in the low silicon-oxygen ratio silicon-based matrix 1, the silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based matrix 1 is 1:1, wherein 1<1≤2, and the silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles 2 is 1:1, wherein 0≤1≤1. The silicon-oxygen ratio is a molar ratio.

[0041] The embodiment of the present invention disperses high silicon-oxygen ratio silicon-based particles in a low silicon-oxygen ratio silicon-based matrix to obtain a silicon-based negative electrode material with different silicon-oxygen concentrations, and the obtained silicon-based negative electrode material has both high capacity and high cycle stability. Among them, the lithium insertion capacity of the high silicon-oxygen ratio silicon-based particles is about 1500-4000mAh / g, which can ensure that the negative electrode material has a high lithium insertion capacity, and the lithium insertion capacity of the low silicon-oxygen ratio silicon-based matrix is ​​about 400-1500mAh / g, which is greater than traditional graphite and amorphous carbon materials. At the same time, since the silicon content of the low silicon-oxygen ratio silicon-based matrix is ​​low and the oxygen content is high, a large volume change will not occur during the lithium insertion process, and the low silicon-oxygen ratio silicon-based matrix is ​​distributed around the high silicon-oxygen ratio silicon-based particles, which can effectively alleviate the volume expansion caused by the high silicon-oxygen ratio silicon-based particles, thereby inhibiting the breakage and pulverization of the silicon-based negative electrode material and improving the cycle life of the silicon-based negative electrode material.

[0042] In one embodiment of the present invention, a low silicon-oxygen ratio silicon-based substrate 1 includes a silicon dioxide 11 substrate and silicon-containing crystal particles 12 dispersed in the silicon dioxide 11 substrate, that is, a silicon oxide system. The silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based substrate 1 can be controlled by controlling the content of the silicon-containing crystal particles 12. Specifically, the silicon-oxygen ratio is 1:11, 1<11<2. In an embodiment of the present invention, the silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based substrate 1 can be, but is not limited to, 1:1.1, 1:1.2, 1:1.3, 1:1.5, 1:1.7, 1:1.8, 1:1.9. In an embodiment of the present invention, the silicon-containing crystal particles can be crystalline silicon and / or lithium-containing silicate. Crystalline silicon can specifically be single crystal silicon or polycrystalline silicon. In an embodiment of the present invention, the silicon-containing crystal particles 12 are uniformly dispersed in the silicon dioxide 11 substrate.

[0043] In another embodiment of the present invention, the low silicon-oxygen ratio silicon-based substrate 1 is silicon dioxide, that is, the silicon-oxygen ratio is 1:2.

[0044] In one embodiment of the present invention, Figure 3 As shown, the high silicon-oxygen ratio silicon-based particles 2 include a silicon dioxide 21 matrix and silicon-containing crystal particles 22 dispersed in the silicon dioxide 21 matrix, that is, a silicon oxide system. The silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles 2 can be controlled by controlling the content of the silicon-containing crystal particles 22. Specifically, the silicon-oxygen ratio is 1:11, 0<11≤1. In an embodiment of the present invention, the silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles 2 can be, for example, 1:0.1, 1:0.2, 1:0.3, 1:0.5, 1:0.7, 1:0.8, 1:1. In an embodiment of the present invention, the silicon-containing crystal particles can be crystalline silicon and / or lithium-containing silicates. In an embodiment of the present invention, the silicon-containing crystal particles 22 are uniformly dispersed in the silicon dioxide 21.

[0045] In another embodiment of the present invention, the high silicon-oxygen ratio silicon-based particles 2 are pure silicon particles, that is, the silicon-oxygen ratio is 1: 0. Pure silicon particles have high capacity, and the pure silicon particles can be single crystal silicon or polycrystalline silicon.

[0046] In the embodiment of the present invention, the low silicon-oxygen ratio silicon-based matrix 1 is a dense structure grown in situ on the surface of the high silicon-oxygen ratio silicon-based particles 2. That is, the low silicon-oxygen ratio silicon-based matrix 1 and the high silicon-oxygen ratio silicon-based particles 2 are not combined in a traditional physical mixing and multi-interface state, but are seamlessly connected into one body without any interface gap, thereby ensuring that the specific surface area of ​​the final silicon-based composite material is as small as possible. In the embodiment of the present invention, the specific surface area of ​​the silicon-based negative electrode material is 0.5-5m 2 / g range.

[0047] In an embodiment of the present invention, the particle size of the high silicon-oxygen ratio silicon-based particles may be 20nm-1000nm. Further, the particle size of the high silicon-oxygen ratio silicon-based particles may be 20nm-500nm, and further, may be 50nm-200nm. Controlling the particle size of the high silicon-oxygen ratio silicon-based particles within a suitable range can better alleviate the volume expansion during the battery cycle while maintaining a high active material gram capacity.

[0048] In an embodiment of the present invention, the particle size of the silicon-containing crystal particles may be 2nm-15nm. Further, the particle size of the silicon-containing crystal particles may be 3nm-10nm. Specifically, for example, it may be 2nm, 3nm, 5nm, 7nm, 10nm, 12nm, 15nm. Silicon-containing crystal particles with a suitable particle size will not cause large volume changes and stresses on the one hand, and can ensure a high degree of ion embedding on the other hand.

[0049] In the embodiment of the present invention, in order to further optimize the material properties, a coating layer can be provided on the surface of the high silicon-oxygen ratio silicon-based particles to achieve different material properties. Specifically, the coating layer can be a conductive material to improve the conductive performance, or an ion conductor material to improve the ion conductivity.

[0050] In one embodiment of the present invention, Figure 3 As shown, the surface of the high silicon-oxygen ratio silicon-based particles is coated with a conductive layer 23. In an embodiment of the present invention, the conductive material of the conductive layer may include but is not limited to one or more of conductive polymers, carbonaceous materials, metals, and alloys. Among them, conductive polymers include but are not limited to polyacetylene, polythiophene, polypyrrole, polyaniline, polyphenylene, polyphenylene ethylene, and polydiyne; carbonaceous materials include but are not limited to amorphous carbon, graphite carbon, carbon fiber, carbon nanotubes, and graphene; metals include but are not limited to Li, Al, Mg, Ti, Cr, Mn, Co, Ni, Cu, and W metals, and alloys may specifically be alloys containing the above metal elements. In an embodiment of the present invention, the thickness of the conductive layer may be 2nm-150nm, further, 10nm-100nm, and further, 50nm-80nm. On the one hand, the conductive layer can improve the conductivity of the silicon-based particles with a high silicon-oxygen ratio, and improve the interface conductivity between the two different silicon-oxygen ratio structures of the silicon-containing matrix and the silicon-based particles; on the other hand, a restriction layer can be formed on the surface of the silicon-based particles with a high silicon-oxygen ratio, effectively reducing the volume expansion caused by lithium insertion and extraction.

[0051] In another embodiment of the present invention, the surface of the high silicon-oxygen ratio silicon-based particles is coated with an ion-conducting layer. In this embodiment of the present invention, the ion conductor material of the ion-conducting layer may include but is not limited to LiPO4, LiLaTiO4, Li7La3Zr2O 12 , LiAlO2, LiAlF4, LiAlS, Li2MgTiO4, Li6La3Zr1.5 W 0.5 O 12 One or more of. In an embodiment of the present invention, the thickness of the ion-conducting layer may be 2nm-150nm, further, may be 10nm-100nm, and further, may be 50nm-80nm. The ion-conducting layer can effectively improve the ion conductivity between two structures with different silicon-oxygen ratios in the negative electrode material. On the one hand, the ion-conducting layer can improve the conductivity of silicon-based particles with high silicon-oxygen ratios, and improve the interface conductivity between two structures with different silicon-oxygen ratios of the silicon-containing matrix and the silicon-based particles; on the other hand, a restriction layer can be formed on the surface of silicon-based particles with high silicon-oxygen ratios, effectively reducing the volume expansion caused by lithium insertion and extraction.

[0052] In other embodiments of the present invention, the surface of the high silicon-oxygen ratio silicon-based particles can also be coated with a conductive layer and an ion-conducting layer at the same time, the conductive layer can be on the inside and the ion-conducting layer can be on the outside, or the ion-conducting layer can be on the inside and the conductive layer can be on the outside.

[0053] The low electrical conductivity of silicon-oxygen materials is an intrinsic defect, and as the oxygen content in the silicon-oxygen structure increases, its electrical conductivity will further decrease, affecting the rapid charge and discharge capability of the material. In an embodiment of the present invention, in order to further improve the electrical conductivity of the material, the silicon-based negative electrode material also includes a carbon coating layer coated on the surface of the low silicon-oxygen ratio silicon-based substrate, and the carbon coating layer constitutes an outer shell. The thickness of the carbon coating layer can be 2nm-2000nm, and further can be 50nm-1000nm. The material of the carbon coating layer can be hard carbon formed by the cracking of a carbon source, or a mixture of hard carbon and carbon nanotubes and / or graphene embedded therein. The surface carbon coating layer can effectively enhance the surface electrical conductivity of the silicon-based composite material and enhance the anti-expansion effect of the particles; at the same time, it can effectively reduce the reaction between the low silicon-oxygen ratio silicon-based substrate and the electrolyte and reduce by-products.

[0054] In the embodiment of the present invention, the particle size of the silicon-based negative electrode material is 3 μm-8 μm, specifically, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm. The suitable particle size range can make the material have a suitable specific surface area, will not consume too much electrolyte, and can also better alleviate volume expansion.

[0055] In the embodiment of the present invention, the shape of the silicon-based negative electrode material is not limited, and can be a regular or irregular shape, such as a spherical shape, a quasi-spherical shape, etc.

[0056] Accordingly, an embodiment of the present invention further provides a method for preparing a silicon-based negative electrode material, comprising:

[0057] S101, mixing silicon powder and silicon dioxide powder at a silicon-oxygen ratio of 1:11, wherein 0<11≤1, and then preparing high silicon-oxygen ratio silicon-based particles by roasting and grinding; or directly using silicon particles as high silicon-oxygen ratio silicon-based particles;

[0058] S102, mixing silicon powder and silicon dioxide powder in a silicon-oxygen ratio of 1:11, wherein 1<11<2, and then calcining them under vacuum or protective atmosphere to form vapor with a low silicon-oxygen ratio; or calcining silicon dioxide powder alone under vacuum or protective atmosphere to form vapor with a low silicon-oxygen ratio;

[0059] S103, depositing the low silicon-oxygen ratio vapor obtained in step S102 on high silicon-oxygen ratio silicon-based particles to form a low silicon-oxygen ratio silicon-based matrix to obtain a silicon-based negative electrode material, wherein the silicon-based negative electrode material includes the low silicon-oxygen ratio silicon-based matrix and high silicon-oxygen ratio silicon-based particles dispersed in the low silicon-oxygen ratio silicon-based matrix.

[0060] In the embodiment of the present invention, in step S101, the calcination operation is performed under vacuum or protective atmosphere, and the calcination temperature may be 1100°C-1600°C, and further, the calcination temperature may be 1200°C-1400°C. In the embodiment of the present invention, the vacuum degree of the vacuum condition may be 10 -3 -10 -1 Pa, the protective atmosphere includes an inert atmosphere or a reducing atmosphere, and specifically can be at least one of a nitrogen atmosphere, a helium atmosphere, an argon atmosphere, and a hydrogen atmosphere.

[0061] In the embodiment of the present invention, step S101 may specifically be: mixing silicon powder and silicon dioxide powder evenly to obtain a mixture, -3 -10 -1 Pa, calcine the mixture at 1100°C-1600°C under vacuum or protective atmosphere, cool and obtain a high silicon-oxygen ratio silicon oxide product; then grind the above product to 20nm-1000nm by liquid phase ball milling or air flow milling to obtain high silicon-oxygen ratio silicon-based particles. The protective atmosphere includes an inert atmosphere or a reducing atmosphere, specifically, at least one of nitrogen, helium, argon and hydrogen atmospheres. After the silicon powder and silicon dioxide powder are mixed, they can be evenly mixed by ball milling.

[0062] In an embodiment of the present invention, when the silicon-containing crystal particles in the high silicon-oxygen ratio silicon-based particles include lithium-containing silicates, step S101 further includes introducing a lithium source during the preparation of the high silicon-oxygen ratio silicon-based particles. The lithium source is specifically a lithium salt. The lithium salt may be one or more of LiH, LiAlH4, Li2CO3, LiNO3, LiAc, and LiOH. The introduction of the lithium source is beneficial to improving the initial charge and discharge efficiency of the battery.

[0063] In the embodiment of the present invention, step S101 may further include: preparing a conductive layer and / or an ion-conducting layer on the surface of high silicon-oxygen ratio silicon-based particles by using a sol-gel method or a vapor deposition method.

[0064] Specifically, the conductive layer can be prepared in the following manner: the high silicon-oxygen ratio silicon-based particles obtained in step S101 are placed in an atmosphere furnace, an organic gas source such as methane, propane, acetylene, etc. is introduced, and vapor deposition is carried out at 750°C-1000°C to obtain high silicon-oxygen ratio silicon-based particles coated with a conductive layer. The thickness of the conductive layer can be 2nm-150nm.

[0065] Specifically, the ion-conducting layer can be prepared in the following manner: the high silicon-oxygen ratio silicon-based particles obtained in step S101 are uniformly mixed with the ion-conducting coating material or the source material of the ion-conducting coating material and a solvent and dried to obtain a mixture; under a protective atmosphere, the mixture is treated at 600°C-1200°C for 0.5-10h to obtain high silicon-oxygen ratio silicon-based particles coated with the ion-conducting layer; the thickness of the ion-conducting layer can be 2nm-150nm.

[0066] In the embodiment of the present invention, in step S102, the calcination temperature for calcining the low silicon-oxygen ratio vapor under vacuum or protective atmosphere is 800°C-1400°C, and the calcination time is 2-40 hours. Further, the calcination time is more than 2 hours, and further, it can be more than 6 hours.

[0067] In an embodiment of the present invention, when the silicon-containing crystal particles in the low silicon-oxygen ratio silicon-based matrix include lithium-containing silicates, step S102 further includes introducing a lithium source during the formation of the low silicon-oxygen ratio vapor. The lithium source is specifically a lithium salt. The lithium salt can be one or more of LiH, LiAlH4, Li2CO3, LiNO3, LiAc, and LiOH. The introduction of the lithium source is beneficial to improving the initial charge and discharge efficiency of the battery.

[0068] In the embodiment of the present invention, in step S103, the specific operation of depositing low silicon-oxygen ratio vapor on high silicon-oxygen ratio silicon-based particles to form a low silicon-oxygen ratio silicon-based matrix is:

[0069] The high silicon-oxygen ratio silicon-based particles are evenly spread on the collector of the high-temperature vacuum furnace, the steam is introduced into the collector of the high-temperature vacuum furnace, and the steam is deposited on the collector of the high-temperature vacuum furnace to form a low silicon-oxygen ratio silicon-based matrix on the high silicon-oxygen ratio silicon-based particles.

[0070] In the embodiment of the present invention, step S103 may further include coating a carbon coating layer on the surface of the low silicon-oxygen ratio silicon-based substrate. Specifically, the carbon coating may be performed by gas phase coating, liquid phase coating or solid phase coating.

[0071] In the embodiment of the present invention, in step S103, after the low silicon-oxygen ratio vapor deposition is completed or after a carbon coating layer is coated on the surface of the low silicon-oxygen ratio silicon-based substrate, further crushing and grinding is performed to obtain a silicon-based negative electrode material with a desired particle size.

[0072] The preparation method provided by the embodiment of the present invention has a simple process and can obtain silicon-based negative electrode materials with different silicon-oxygen concentration confined distributions, so that the silicon-based negative electrode materials have both high capacity and high cycle stability.

[0073] The embodiment of the present invention further provides a battery, comprising a positive electrode plate, a negative electrode plate, a separator, and an electrolyte, wherein the negative electrode plate comprises a negative electrode active material, and the negative electrode active material comprises the negative electrode material provided in the embodiment of the present invention. The battery may be a lithium-ion battery. The battery provided in the embodiment of the present invention has a high capacity and good cycle performance, and can be used in terminal consumer products, such as mobile phones, tablet computers, portable computers, notebook computers, and other wearable or portable electronic devices.

[0074] like Figure 4 As shown, an embodiment of the present invention further provides a terminal 200, which can be a mobile phone, or an electronic product such as a tablet computer, a laptop computer, a portable machine, a smart wearable product, etc. The terminal 200 includes a shell 201 assembled on the outside of the terminal, and a circuit board and a battery (not shown in the figure) located inside the shell 201. The battery is electrically connected to the circuit board to power the circuit board, wherein the battery is the battery provided in the above-mentioned embodiment of the present invention, and the shell 201 may include a front cover assembled on the front side of the terminal and a rear shell assembled on the rear side, and the battery may be fixed on the inside of the rear shell.

[0075] The embodiments of the present invention are further described below with reference to a plurality of embodiments.

[0076] Example 1

[0077] (1) Silicon powder and silicon dioxide powder (the molar ratio of silicon to oxygen is controlled to be 2:1) are mixed and ball milled for 3 h at a speed of 350 rpm to obtain a mixture after mixing evenly; -3 -10 -1 Pa, in a vacuum environment, calcining the mixture at 1250° C. for 6 hours, and rapidly cooling to obtain a high silicon-oxygen ratio silicon oxide precipitate; then grinding the high silicon-oxygen ratio silicon oxide precipitate to a particle size of about 200 nm by liquid phase ball milling or air flow milling to obtain high silicon-oxygen ratio silicon-based particles;

[0078] (2) placing the high silicon-oxygen ratio silicon-based particles obtained above into an atmosphere furnace, introducing methane, and vapor deposition at 750-1000° C., crushing the product after the deposition is completed to obtain carbon-coated high silicon-oxygen ratio silicon-based particles with a size of about 200 nm; and then evenly spreading the obtained carbon-coated high silicon-oxygen ratio silicon-based particles on a collector of a high-temperature vacuum furnace;

[0079] (3) Silicon powder and silicon dioxide powder (the molar ratio of silicon to oxygen is controlled to be 1:1.5) are mixed and ball milled at 350 rpm for 3 h to obtain a mixture; -3-10 -1 Pa, in a vacuum environment, calcining the mixture at 1250° C. for 6 hours to obtain silicon-oxygen vapor; passing the silicon-oxygen vapor into a high-temperature vacuum furnace, depositing the silicon-oxygen vapor on the surface of carbon-coated silicon-based particles with a high silicon-oxygen ratio to form a low silicon-oxygen ratio silicon-based matrix, and crushing the particles to a particle size of 3-8 μm;

[0080] (4) placing the product obtained in step (3) into an atmosphere furnace, introducing methane, and causing vapor deposition at 750-1000° C. to form a carbon coating layer on the surface of the product, thereby obtaining a silicon-based negative electrode material.

[0081] Figure 5 This is a SEM image of the silicon-based negative electrode material prepared in Example 1 of the present invention. It can be seen from the image that the particle size of the silicon-based negative electrode material is basically 3μm-8μm. Fig. 6A 1 is a cross-sectional SEM image of a silicon-based negative electrode material, in which 1 is a low silicon-oxygen ratio silicon-based substrate, 2 is a high silicon-oxygen ratio silicon-based particle, and 3 is a carbon coating layer on the surface of the low silicon-oxygen ratio silicon-based substrate; Figure 6B for Fig. 6A A magnified image of a silicon-based substrate with a low silicon-oxygen ratio in region A, where the dark black aggregates in the white box are silicon-containing crystal particles; Figure 6C for Fig. 6A The enlarged image of the silicon-based particles with high silicon-oxygen ratio in the middle B area, where 22 is a silicon-containing crystal particle; Figure 6B , Figure 6C It can be seen from the two figures that both the low silicon-oxygen ratio silicon-based matrix and the high silicon-oxygen ratio silicon-based particles are composed of silicon-containing crystal particles dispersed in the silicon dioxide matrix. The difference lies in the different distribution density and quantity of the silicon-containing crystal particles, which results in different silicon-oxygen ratios.

[0082] Example 2

[0083] (1) Under a protective atmosphere, single crystal silicon is ball-milled to a particle size of about 200 nm to obtain high silicon-oxygen ratio silicon-based particles;

[0084] (2) placing the high silicon-oxygen ratio silicon-based particles obtained above into an atmosphere furnace, introducing methane, and vapor deposition at 750-1000° C., crushing the product to ensure that the particle size is about 200 nm, and forming carbon-coated high silicon-oxygen ratio silicon-based particles; and evenly spreading the carbon-coated high silicon-oxygen ratio silicon-based particles on a collector of a high-temperature vacuum furnace;

[0085] (3) Silicon powder and silicon dioxide powder (the molar ratio of silicon to oxygen is controlled to be 1:1.5) are mixed and ball-milled at 350 rpm for 3 h to obtain a uniform mixture; -3 -10 -1The mixture was calcined at 1250°C for 6 hours under a Pa vacuum environment to obtain silicon-oxygen vapor with a low silicon-oxygen ratio; the silicon-oxygen vapor was introduced into a high-temperature vacuum furnace, and the silicon-oxygen vapor was deposited on the surface of carbon-coated silicon-based particles with a high silicon-oxygen ratio to form a silicon-based matrix with a low silicon-oxygen ratio, and the particles were crushed to a particle size of 3-8 μm;

[0086] (4) placing the product obtained in step (3) into an atmosphere furnace, introducing methane, and causing vapor deposition at 750-1000° C. to form a carbon coating layer on the surface of the product, thereby obtaining a silicon-based negative electrode material.

[0087] Example 3

[0088] (1) Under a protective atmosphere, single crystal silicon is ball-milled to a particle size of about 200 nm to obtain high silicon-oxygen ratio silicon-based particles;

[0089] (2) placing the obtained high silicon-oxygen ratio silicon-based particles into an atomic layer deposition device, and depositing Li3PO4 under vacuum or inert atmosphere to form Li3PO4-coated high silicon-oxygen ratio silicon-based particles, wherein the thickness of the Li3PO4 coating layer is 8-15 nm; and evenly spreading the Li3PO4-coated high silicon-oxygen ratio silicon-based particles on a collector of a high-temperature vacuum furnace;

[0090] (3) Silicon powder and silicon dioxide powder (the molar ratio of silicon to oxygen is controlled to be 1:1.5) are mixed and ball-milled at 350 rpm for 3 h to obtain a uniform mixture; -3 -10 -1 Under a vacuum environment of Pa, the mixture is calcined at 1250°C for 6 hours to obtain silicon-oxygen vapor with a low silicon-oxygen ratio; the silicon-oxygen vapor is passed into a high-temperature vacuum furnace, and the silicon-oxygen vapor is deposited on the surface of silicon-based particles with a high silicon-oxygen ratio coated with Li3PO4 to form a silicon-based matrix with a low silicon-oxygen ratio, and the particles are crushed to a particle size of 3-8 μm;

[0091] (4) placing the product obtained in step (3) into an atmosphere furnace, introducing methane, and vapor deposition at 750-1000° C. to form a carbon coating layer on the surface of the product, thereby obtaining a low-expansion silicon-based negative electrode material.

[0092] Comparative Example 1:

[0093] (1) SiO with a particle size of about 200 nm 1.1 The powder (silicon particles uniformly distributed in a silicon dioxide matrix) is dispersed in an ethanol solution, mixed evenly, and the solid content is controlled to be about 25% to form a slurry;

[0094] (2) adding natural graphite particles with a particle size of 5-20 μm to the above slurry, mixing evenly, and drying to obtain a mixture;

[0095] (3) placing the mixture under a protective atmosphere, heating it to 850-1000° C. at a heating rate of 3-5° C. / min, keeping the temperature for 3-5 hours, and cooling it to room temperature to obtain a composite;

[0096] (4) The above-mentioned composite material is crushed to obtain a silicon-oxygen / carbon composite material with a particle size of 3-8 μm.

[0097] The silicon-based negative electrode materials prepared in Examples 1, 2 and 3 of the present invention, and the silicon-oxygen / carbon composite material prepared in Comparative Example 1 were mixed with graphite in a certain proportion to prepare negative electrode materials with a gram capacity of 500 mAh / g, and matched with the positive electrode material lithium cobalt oxide to prepare soft-packed batteries and test the electrochemical performance. According to the same test system, the expansion of the electrode sheet in the fully charged state of the battery was tested, and the expansion of the battery was measured after 600 charge and discharge cycles. The results are shown in Table 1:

[0098] Table 1 Performance comparison between the embodiment of the present invention and comparative example 1

[0099]

[0100] It can be seen from the results in Table 1 that the battery prepared by using the silicon-based negative electrode material of the embodiment of the present invention has a significantly improved cycle performance compared to the battery prepared by the existing traditional silicon-oxygen / carbon composite negative electrode material. The expansion rate of the electrode sheet is significantly reduced when fully charged, and the expansion rate of the battery cell is significantly reduced after 600 cycles. This is because the silicon-based negative electrode material of the embodiment of the present invention achieves a confined distribution of different silicon-oxygen concentrations by dispersing high silicon-oxygen ratio silicon-based particles in a low silicon-oxygen ratio silicon-based matrix, and the resulting silicon-based negative electrode material takes into account both high capacity and high cycle stability. Among them, the high silicon-oxygen ratio silicon-based particles can ensure that the negative electrode material has a high lithium insertion capacity, while the low silicon-oxygen ratio silicon-based matrix will not produce a large volume change during the lithium insertion process, and the low silicon-oxygen ratio silicon-based matrix is ​​distributed around the high silicon-oxygen ratio silicon-based particles, which can effectively alleviate the volume expansion caused by the high silicon-oxygen ratio silicon-based particles, thereby inhibiting the breakage and pulverization of the silicon-based negative electrode material and improving the cycle life of the silicon-based negative electrode material. In addition, the provision of a conductive layer on the surface of high silicon-oxygen ratio silicon-based particles can improve the electrical conductivity of high silicon-oxygen ratio silicon-based particles, and improve the interface conductivity between two structures with different silicon-oxygen ratios, the silicon-containing matrix and the silicon-based particles; at the same time, a restriction layer can be formed on the surface of high silicon-oxygen ratio silicon-based particles, effectively reducing the volume expansion caused by lithium insertion and extraction.

Claims

1. A silicon-based negative electrode material, characterized in that: It includes a low silicon-oxygen ratio silicon-based matrix, and a plurality of high silicon-oxygen ratio silicon-based particles dispersed in the low silicon-oxygen ratio silicon-based matrix. The silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based matrix is 1:x, where 1 < x ≤ 2, and the silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles is 1:y, where 0 ≤ y ≤ 1; an ion-conducting layer is provided on the surface of the high silicon-oxygen ratio silicon-based particles.

2. The silicon-based negative electrode material according to claim 1, characterized in that: The low silicon-oxygen ratio silicon-based matrix is silica, or the low silicon-oxygen ratio silicon-based matrix includes silica and silicon-containing crystal particles dispersed in the silica, and the low silicon-oxygen ratio silicon-based matrix is distributed around the high silicon-oxygen ratio silicon-based particles.

3. The silicon-based negative electrode material according to claim 1, characterized in that: The high silicon-oxygen ratio silicon-based particles are silicon particles, or the high silicon-oxygen ratio silicon-based particles include silica and silicon-containing crystal particles dispersed in the silica.

4. The silicon-based negative electrode material according to any one of claims 1 to 3, characterized in that: The low silicon-oxygen ratio silicon-based matrix is in-situ grown on the surface of the high silicon-oxygen ratio silicon-based particles.

5. The silicon-based negative electrode material according to claim 2 or 3, characterized in that: The silicon-containing crystal particles are crystalline silicon and / or lithium-containing silicate.

6. The silicon-based negative electrode material according to claim 2 or 3, characterized in that: The particle size of the silicon-containing crystal particles is 2 nm - 15 nm.

7. The silicon-based negative electrode material according to any one of claims 1 to 3, characterized in that: The particle size of the high silicon-oxygen ratio silicon-based particles is 20 nm - 1000 nm.

8. The silicon-based negative electrode material according to any one of claims 1 to 3, characterized in that: A conductive layer is further provided on the surface of the high silicon-oxygen ratio silicon-based particles.

9. The silicon-based negative electrode material according to claim 8, characterized in that: The surface of the high silicon-oxygen ratio silicon-based particles is coated with both the conductive layer and the ion-conducting layer at the same time, where the conductive layer is on the inner side and the ion-conducting layer is on the outer side, or the ion-conducting layer is on the inner side and the conductive layer is on the outer side.

10. The silicon-based negative electrode material according to claim 8, characterized in that: The material of the conductive layer is selected from one or more of conductive polymers, carbonaceous materials, metals, and alloys.

11. The silicon-based negative electrode material according to claim 1, characterized in that: The material of the ion-conducting layer is selected from LiPO4, LiLaTiO4, Li7La3Zr2O 12 , LiAlO2, LiAlF4, LiAlS, Li2MgTiO4, Li6La3Zr 1.5 W 0.5 O 12 One or more of .

12. The silicon-based negative electrode material according to claim 8, characterized in that: The thickness of the conductive layer is 2 nm - 150 nm, and the thickness of the ion-conducting layer is 2 nm - 150 nm.

13. The silicon-based negative electrode material according to any one of claims 1 to 3, characterized in that: The silicon-based anode material further includes a carbon coating layer coated on the surface of the low silicon-oxygen ratio silicon-based matrix.

14. The silicon-based negative electrode material according to any one of claims 1 to 3, characterized in that: The particle size of the silicon-based anode material is 3 μm - 8 μm.

15. A method for preparing a silicon-based negative electrode material, characterized in that: It includes: Mix silicon powder and silica powder according to a silicon-oxygen ratio of 1:y1, where 0 < y1 ≤ 1, and then prepare high silicon-oxygen ratio silicon-based particles through roasting and grinding; or directly use silicon particles as the high silicon-oxygen ratio silicon-based particles; use the sol-gel method or chemical vapor deposition method to prepare an ion-conducting layer on the surface of the high silicon-oxygen ratio silicon-based particles; Mix silicon powder and silica powder according to a silicon-oxygen ratio of 1:x1, where 1 < x1 < 2, and then roast in a vacuum or protective atmosphere to form a low silicon-oxygen ratio vapor; or roast silica powder alone in a vacuum or protective atmosphere to form a low silicon-oxygen ratio vapor; Deposit the low silicon-oxygen ratio vapor on the high silicon-oxygen ratio silicon-based particles with an ion-conducting layer on the surface to form a low silicon-oxygen ratio silicon-based matrix, obtaining a silicon-based anode material. The silicon-based anode material includes a low silicon-oxygen ratio silicon-based matrix, and a plurality of high silicon-oxygen ratio silicon-based particles dispersed in the low silicon-oxygen ratio silicon-based matrix. The silicon-oxygen ratio of the low silicon-oxygen ratio silicon-based matrix is 1:x, where 1 < x ≤ 2, and the silicon-oxygen ratio of the high silicon-oxygen ratio silicon-based particles is 1:y, where 0 ≤ y ≤ 1; an ion-conducting layer is provided on the surface of the high silicon-oxygen ratio silicon-based particles.

16. The preparation method according to claim 15, characterized in that: The low silicon-oxygen ratio silicon-based matrix is silica, or the low silicon-oxygen ratio silicon-based matrix includes silica and silicon-containing crystal particles dispersed in the silica.

17. The preparation method according to claim 15, characterized in that: The high silicon-oxygen ratio silicon-based particles are silicon particles, or the high silicon-oxygen ratio silicon-based particles include silicon dioxide and silicon-containing crystal particles dispersed in the silicon dioxide.

18. The preparation method according to claim 15, characterized in that: The preparation method further comprises: A conductive layer is prepared on the surface of the high silicon-oxygen ratio silicon-based particles by using a sol-gel method or a vapor deposition method.

19. The preparation method according to claim 15, characterized in that: In the step of calcining and grinding to prepare silicon-based particles with a high silicon-oxygen ratio, the calcination is carried out under vacuum or protective atmosphere at a calcination temperature of 1100°C-1600°C.

20. The preparation method according to claim 15, characterized in that: In the step of baking under vacuum or protective atmosphere to form steam with a low silicon-oxygen ratio, the baking temperature is 800° C.-1400° C. and the baking time is 2-40 hours.

21. The preparation method according to claim 17, characterized in that: When the silicon-containing crystalline particles in the high silicon-oxygen ratio silicon-based particles include lithium-containing silicate, the preparation method further comprises introducing a lithium source during the preparation of the high silicon-oxygen ratio silicon-based particles.

22. The preparation method according to claim 16, characterized in that: When the silicon-containing crystal particles in the low silicon-oxygen ratio silicon-based matrix include lithium-containing silicate, the preparation method further comprises introducing a lithium source during the formation of the low silicon-oxygen ratio vapor.

23. The preparation method according to claim 15, characterized in that: The preparation method further comprises: forming a carbon coating layer on the surface of the low silicon-oxygen ratio silicon-based substrate.

24. A battery, characterized in that: It includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte, wherein the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes the silicon-based negative electrode material as described in any one of claims 1-14.

25. A terminal, characterized in that: It comprises a terminal shell, and a circuit board and a battery located inside the terminal shell, wherein the battery is electrically connected to the circuit board for supplying power to the circuit board, and the battery comprises the battery according to claim 24.

Citation Information

Cited By

  • Integrated preparation method of silicon-based composite powder material

    CN120590065A