Catalyst for ammonia decomposition reaction and hydrogen production method using the catalyst

By using shape-controlled cerium oxide catalyst carriers and metal oxide composites, combined with catalyst enhancers, the problem of low conversion rate and instability of existing ammonia decomposition catalysts is solved, and efficient ammonia decomposition and hydrogenation at lower temperatures are achieved. production, with long-term stability.

CN116056789BActive Publication Date: 2024-10-25KOREA RES INST OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180054864.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-16
Filing Date
2021-09-07
Publication Date
2024-10-25
Estimated Expiration
2041-09-07

AI Technical Summary

Technical Problem

Existing ammonia decomposition catalysts have low and unstable conversion rates in ammonia decomposition reactions, making it difficult to achieve efficient ammonia decomposition at lower temperatures. High-purity hydrogen production requires high reaction temperatures, which affects the application of hydrogen energy.

Method used

Cerium oxides in the shape of cubes and spindles are used as catalyst carriers, combined with specific metal oxide complexes and catalyst enhancers, to improve catalyst activity and stability through shape control and composition design.

Benefits of technology

It significantly improves the ammonia conversion rate at lower temperatures and maintains catalyst activity during long-term reactions, achieving efficient ammonia decomposition and hydrogen production with long-term stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116056789B_ABST
    Figure CN116056789B_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst for an ammonia decomposition reaction and a method for producing hydrogen using the catalyst, and more particularly to a catalyst for an ammonia decomposition reaction which can improve the ammonia conversion rate and exhibit long-term stability during the ammonia decomposition reaction by controlling the shape of a cerium oxide used as a catalyst carrier during the ammonia decomposition reaction and containing cesium as a catalyst enhancer, and a method for producing hydrogen using the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalyst for an ammonia decomposition reaction and a method for producing hydrogen using the catalyst, and in particular to a catalyst for an ammonia decomposition reaction which can improve an ammonia conversion rate in the ammonia decomposition reaction and exhibit long-term stability, and a method for producing hydrogen using the catalyst. Background Art

[0002] With the recent intensification of climate change, hydrogen energy has attracted worldwide attention as an environmentally friendly alternative to fossil fuels. In order to realize the practical application of hydrogen energy, it is crucial to develop a technology that can safely and efficiently store and transport hydrogen. Although there are many methods for storing hydrogen, as a hydrogen storage medium installed in fuel cell vehicles, the method of using a hydrogen storage material that can reversibly store and release hydrogen is highly anticipated.

[0003] As hydrogen storage materials, there are liquid hydrogen storage materials using hydrogen storage alloys or organic compounds, and as a means of simply obtaining hydrogen, there is a method using an ammonia decomposition reaction.

[0004] In addition, since ammonia has a foul odor, especially a pungent odor, it needs to be treated when the content in the gas exceeds the odor threshold. Therefore, various ammonia treatment methods have been studied. For example, there are methods of oxidizing ammonia into nitrogen and water by contacting ammonia with oxygen and methods of decomposing ammonia into nitrogen and hydrogen.

[0005] Patent Document 1 discloses an ammonia treatment method in which nickel or nickel oxide is supported on a metal oxide carrier such as alumina, silica, titania, and zirconia, and a catalyst to which at least one of alkaline earth metals and lanthanide elements is added in the form of a metal or an oxide is used in the process of decomposing ammonia generated in a process of treating organic waste into nitrogen and hydrogen. However, the ammonia treatment method described above is not practical because the decomposition rate of ammonia is low.

[0006] In addition, a method of using hydrogen recovered by decomposing ammonia as a hydrogen source for a fuel cell has recently been studied, but in the above case, high-purity hydrogen is required. If high-purity hydrogen is to be obtained using ammonia decomposition catalysts that have been proposed, a high reaction temperature (>500°C) must be reached to overcome a high activation barrier (Patent Document 2).

[0007] In order to solve the above problems, people are committed to developing various catalysts that use cerium oxide (CeO2) as a catalyst carrier that can decompose ammonia at a lower temperature and a higher conversion rate. In particular, the catalyst carrier with controlled shape can control the ratio of the surface area to the volume exposed on the surface, the type and ratio of the exposed crystal surface, and these changes will have a significant impact on the activity of the catalyst.

[0008] However, there are few research activities on using cerium oxide catalyst supports as catalysts in ammonia decomposition reactions by introducing them, and they have not yet reached the stage of commercialization.

[0009] Patent Document 1: Japanese Patent Publication No. 2004-195454 (publication date: July 15, 2004)

[0010] Patent Document 2: Korean Patent Gazette No. 1781412 (Publication Date: September 25, 2017) Summary of the invention

[0011] The main object of the present invention is to solve the above-mentioned problems and provide a catalyst for an ammonia decomposition reaction which can improve the ammonia conversion rate in the ammonia decomposition reaction and exhibit long-term stability, and a method for producing hydrogen using the catalyst.

[0012] In order to achieve the above-mentioned purpose, an implementation example of the present invention provides a catalyst for ammonia decomposition reaction, characterized in that the catalyst is a catalyst for ammonia decomposition reaction comprising a catalyst carrier and a catalytic active substance loaded on the catalyst carrier, and the catalyst carrier is a cerium oxide in one or more shapes selected from the group consisting of a cube shape and a spindle shape.

[0013] A preferred embodiment of the present invention is characterized in that the catalytically active material is one or more selected from the group consisting of ruthenium, nickel, molybdenum, iron and cobalt.

[0014] A preferred embodiment of the present invention is characterized in that the catalyst for ammonia decomposition reaction contains 0.1 wt% to 50 wt% of a catalyst active substance relative to the total weight of the catalyst for ammonia decomposition reaction.

[0015] A preferred embodiment of the present invention is characterized in that the catalyst carrier is a metal oxide complex of one or more metal oxides selected from lanthanum (La), yttrium (Y), praseodymium (Pr), neodymium (Nd), samarium (Sm) and gadolinium (Gd) and cerium oxide.

[0016] A preferred embodiment of the present invention is characterized in that, in the metal oxide composite, the molar ratio of cerium to the metal other than cerium is 40:60 to 95:5.

[0017] A preferred embodiment of the present invention is characterized in that the size of the cubic particles is less than 1 μm.

[0018] A preferred embodiment of the present invention is characterized in that the catalyst for ammonia decomposition reaction contains one or more catalyst enhancers selected from the group consisting of cesium and potassium.

[0019] A preferred embodiment of the present invention is characterized in that the catalyst for ammonia decomposition reaction contains 0.01 wt% to 25 wt% of a catalyst enhancer relative to the total weight of the catalyst for ammonia decomposition reaction.

[0020] Another implementation example of the present invention provides a method for producing hydrogen from ammonia using the catalyst for ammonia decomposition reaction.

[0021] Another preferred embodiment of the present invention is characterized in that the ammonia decomposition reaction is performed within a temperature range of 300°C to 500°C.

[0022] The catalyst for ammonia decomposition reaction according to the present invention controls the shape of cerium oxide used as a catalyst carrier in the ammonia decomposition process and contains a catalyst enhancer, thereby ensuring excellent catalyst activity during the ammonia decomposition reaction and improving the ammonia conversion rate. Even after a long period of reaction at a relatively high temperature, there is no significant decrease in activity, so it has excellent long-term stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 These are transmission electron microscope (TEM) photographs of catalyst 1 and catalyst 5 of the present invention, wherein (a) is a transmission electron microscope (TEM) photograph of catalyst 1, (b) is a photograph of (a) magnified 20 times, (c) is a transmission electron microscope (TEM) photograph of catalyst 5, and (d) is a photograph of (c) magnified 2 times.

[0024] Figure 2 These are transmission electron microscope (TEM) photographs of catalyst 6 and catalyst 7 of the present invention, wherein (a) is a transmission electron microscope (TEM) photograph of catalyst 6, (b) is a photograph of (a) enlarged by 4 times, (c) is a transmission electron microscope (TEM) photograph of catalyst 7, and (d) is a photograph of (c) enlarged by 10 times.

[0025] Figure 3This is a graph showing the results of measuring the ammonia decomposition activity when the content of the catalyst enhancer of the present invention is changed.

[0026] Figure 4 This is a graph showing the results of measuring the long-term stability of the catalyst produced by the catalyst of the present invention and the catalyst 8.

[0027] Figure 5 This is a comparative chart illustrating the results of hydrogen temperature programmed reduction (H2-TPR) analysis of some catalysts of the present invention.

[0028] Figure 6 This is a comparative graph illustrating the results of hydrogen temperature programmed reduction (H2-TPR) analysis of catalysts when the content of the catalyst enhancer of the present invention is changed. DETAILED DESCRIPTION

[0029] Unless otherwise defined, the meaning of all technical and scientific terms used in this specification is the same as that commonly understood by a skilled professional in the technical field to which the present invention belongs. Generally speaking, the nomenclature used in this specification is well known and commonly used in the technical field.

[0030] The terms such as "equipped with", "including" or "having" recorded in this specification are only used to indicate the existence of the features, values, steps, actions, constituent elements, parts or the combination described in the specification, and do not exclude in advance the possibility that other features, values, steps, actions, constituent elements, parts or the combination not mentioned exist or are added.

[0031] One aspect of the present invention relates to a catalyst for an ammonia decomposition reaction, characterized in that the catalyst is a catalyst for an ammonia decomposition reaction comprising a catalyst carrier and a catalytically active substance supported on the catalyst carrier, and the catalyst carrier is a cerium oxide having one or more shapes selected from a group consisting of a cube shape and a spindle shape.

[0032] There are few research activities on the application of nanoparticle catalyst supports to the ammonia decomposition reaction, and they have not yet reached the stage of commercialization. In particular, there is no research activity on controlling the shape of the catalyst support to change the specific exposed crystal faces and the crystal face surface ratio to enhance the ammonia dehydrogenation reaction.

[0033] Therefore, the present inventors confirmed that in the ammonia dehydrogenation reaction, the catalyst activity differs depending on the catalyst carrier whose shape is controlled regardless of the specific surface area of ​​the catalyst carrier, and surprisingly found that by introducing a catalyst enhancer of a specific component into the cerium oxide catalyst carrier whose shape is controlled, ammonia can be decomposed with higher activity than in the past, thereby completing the present invention.

[0034] Generally speaking, lattice oxygen exists in metal oxides, and the lattice oxygen has extremely high reactivity depending on its type and shape, and also affects the conductivity of the catalyst due to the movement of oxygen or electrons in the lattice structure.

[0035] In particular, cerium is a rare earth metal that exhibits high electrical conductivity, and for cerium oxide whose particle shape is controlled to be a cube and / or a spindle shape, the agglomeration effect of the catalyst active material particles can be limited by the interaction between the catalyst active material and the carrier in the high-temperature ammonia dehydrogenation reaction, and sufficient electron density can be provided for the catalyst active material. Thus, the cerium oxide whose particle shape is controlled to be a cube and / or a spindle shape can improve the catalyst activity by changing the electron density of the active region of the catalyst active material, and can also improve thermal stability and durability.

[0036] As a method for manufacturing the catalyst carrier with controlled shape, any method that can shape the particles into a cubic and / or spindle shape can be applied without restriction. As an example, it can be manufactured by methods such as hydrothermal synthesis, precipitation method, polyol method, metal ion reduction method and electrochemical deposition method.

[0037] The size of the cubic particles may be less than 1 μm, preferably 5 nm to 100 nm, more preferably 10 nm to 30 nm, and most preferably 12 nm to 18 nm. If the size of the cubic particles exceeds 1 μm, the catalyst activity enhancement effect according to the present invention will not be significant.

[0038] In addition, the catalyst carrier of the present invention can be a metal oxide composite in which one or more metal oxides selected from lanthanum (La), yttrium (Y), praseodymium (Pr), neodymium (Nd), samarium (Sm) and gadolinium (Gd) are compounded with cerium oxide, and the shape of the composite metal oxide can be a cubic and / or spindle shape.

[0039] In the composite metal oxide composite, the molar percentage of cerium may be 40 mol% to 95 mol%, preferably 50 mol% to 90 mol%.

[0040] As a method for manufacturing the catalyst carrier with controlled shape, any method that can shape the particles into a cubic and / or spindle shape can be applied without restriction. As an example, it can be manufactured by methods such as hydrothermal synthesis, precipitation method, polyol method, metal ion reduction method and electrochemical deposition method.

[0041] Furthermore, the catalytically active material supported on the catalyst carrier may be one or more selected from the group consisting of ruthenium, nickel, molybdenum, iron, and cobalt, and preferably may be ruthenium.

[0042] Generally speaking, there is a certain tendency between the degree of electron filling in the D-band of the metal used as a catalytic active substance and the adsorption energy between nitrogen and the metal, and there is also a tendency between this and the efficiency of ammonia dehydrogenation. Specifically, the more electrons filled in the D-band, the lower the adsorption energy between the catalytic active substance and nitrogen becomes, and the fewer electrons filled, the higher the adsorption energy between the catalytic active substance and nitrogen becomes. Among them, when ruthenium is used as a catalytic active substance, it has the smallest nitrogen adsorption energy, but it cannot be said to be the best. Therefore, in the present invention, the electron density in the D-band of ruthenium can be changed by using cerium oxide with controlled shape as a carrier, so that a specific metal oxide has the best nitrogen binding energy and thereby improves the ammonia dehydrogenation activity.

[0043] The catalyst active material may be loaded in an amount of 0.1 wt % to 50 wt % relative to the total weight of the catalyst. If the loaded catalyst active material is less than 0.1 wt %, it may be difficult to achieve the effect of improving the performance, and if it exceeds 50 wt %, the performance of the catalyst may be reduced due to agglomeration between the catalyst active materials.

[0044] In addition, the catalyst for ammonia decomposition reaction according to the present invention may include one or more catalyst enhancers selected from the group consisting of cesium and potassium. The catalyst enhancer can provide electrons to ruthenium (Ru) and other catalyst active materials in the ammonia decomposition reaction to increase the electron density thereof, thereby enabling the dissociated adsorbed nitrogen to be more effectively separated into nitrogen molecules in an important step of the ammonia decomposition reaction and thereby improving the efficiency of the ammonia decomposition reaction.

[0045] The content of the catalyst enhancer can be determined in consideration of the content of the catalytically active substance, and preferably 0.01 wt% to 25 wt%, more preferably 0.5 wt% to 10 wt%, relative to the total weight of the catalyst. If the content of the catalyst enhancer is less than 0.01 wt%, it may be difficult to achieve a catalyst promotion effect, and if it exceeds 25 wt%, the catalyst activity may not be enhanced to a high degree compared to the content.

[0046] The catalyst for ammonia decomposition reaction according to the present invention as described above can be applied without limitation to a method in which the catalyst active substance or the catalyst active substance and the catalyst enhancer are loaded onto the catalyst carrier by heat treatment after reacting the catalyst carrier and the catalyst active substance precursor or the catalyst carrier and the catalyst active substance precursor and the catalyst enhancer precursor. As an example, it can include deposition-precipitation (DP) method, dry impregnation method, wet impregnation method, sol-gel method, hydrothermal synthesis method and polyol method, etc.

[0047] At this time, the catalyst active material precursor can be one or more selected from the group consisting of organic compounds and inorganic compounds containing catalyst active material ions, specifically, it can be chloride, hydrate, nitride, acetylacetonate and iodide of the catalyst active material.

[0048] In addition, the precursor of the catalyst enhancer can be one or more selected from the group consisting of organic compounds and inorganic compounds containing catalyst enhancer ions, specifically, it can be hydroxide, chloride, nitride, carbonate, fluoride and acetate of cesium or potassium.

[0049] The catalyst activity, thermal stability and durability of the catalyst for ammonia decomposition reaction as described above are all improved, so that the ammonia conversion rate can be improved in the ammonia decomposition reaction, and long-term stability can be exhibited even at higher temperatures and for longer periods of time.

[0050] Another aspect of the present invention relates to a method for producing hydrogen from ammonia using the catalyst for ammonia decomposition reaction.

[0051] According to the hydrogen production method of the present invention, a catalyst for ammonia decomposition reaction using cube-shaped and / or spindle-shaped cerium oxide as a catalyst carrier can be used to treat ammonia-containing gas and dehydrogenate the ammonia into nitrogen and hydrogen, thereby producing hydrogen.

[0052] The catalyst for ammonia decomposition reaction can exhibit an ammonia conversion rate of more than 80% at a temperature ranging from 400°C to 500°C, and specifically, can exhibit an ammonia conversion rate of more than 96% at a temperature ranging from 450°C to 500°C.

[0053] Next, the present invention will be described in more detail by way of specific examples. The following examples are only examples to help understand the present invention, and the scope of the present invention is not limited thereby.

[0054] <Carrier 1: Cube-shaped ceria catalyst carrier>

[0055] A solution of 12.0 g of NaOH (97%, Daejung) added to 40 ml of deionized water was added dropwise to a solution of 1.3 g of Ce(NO3)3·6H2O (Sigma, 99%) dissolved in 30 ml of distilled water. Next, the solution was mixed in a 100 ml polytetrafluoroethylene bottle and stirred continuously for 30 minutes. Finally, the polytetrafluoroethylene bottle was completely sealed and heated at 160°C for 24 hours in a stainless steel container autoclave. Next, the resulting precipitate was collected and washed several times with deionized water and ethanol, then dried in an oven at 80°C for 24 hours, and then sintered at 500°C for 4 hours to obtain a cubic CeO2 catalyst carrier with a particle size of 15 nm.

[0056] <Carrier 2: Cube-shaped ceria catalyst carrier>

[0057] A solution of 12 g of NaOH (97%, Daejung) added to 40 ml of deionized water was added dropwise to a solution of 0.65 g of Ce(NO3)3·6H2O (Sigma, 99%) dissolved in 30 ml of distilled water. Next, the solution was mixed in a 100 ml polytetrafluoroethylene bottle and stirred continuously for 30 minutes. Finally, the polytetrafluoroethylene bottle was completely sealed and heated at 160°C for 24 hours in a stainless steel container autoclave. Next, the resulting precipitate was collected and washed several times with deionized water and ethanol, then dried in an oven at 80°C for 24 hours, and then calcined at 500°C for 4 hours to obtain a cubic CeO2 catalyst carrier with a particle size of 10 nm.

[0058] <Carrier 3: Cube-shaped ceria catalyst carrier>

[0059] A solution of 12 g of NaOH (97%, Daejung) added to 40 ml of deionized water was added dropwise to a solution of 2.6 g of Ce(NO3)3·6H2O (Sigma, 99%) dissolved in 30 ml of distilled water. Next, the solution was mixed in a 100 ml polytetrafluoroethylene bottle and stirred continuously for 30 minutes. Finally, the polytetrafluoroethylene bottle was completely sealed and heated at 160°C for 24 hours in a stainless steel container autoclave. Next, the generated precipitate was collected and washed several times with deionized water and ethanol, then dried in an oven at 80°C for 24 hours, and then calcined at 500°C for 4 hours to obtain a cubic CeO2 catalyst carrier with a particle size of 20 nm.

[0060] <Carrier 4: Spindle-shaped cerium oxide catalyst carrier>

[0061] 2.6 g of Ce(NO3)3·6H2O (Sigma, 99%) and 1 g of urea (Samchun, 99%) were dissolved in 70 ml of deionized water. After the mixture was moved to a 100 ml Teflon-lined autoclave, it was heated to 120°C and then maintained at the temperature for 8 hours. Next, the resulting precipitate was collected and washed several times with deionized water and ethanol, and then dried in a vacuum oven at 80°C for 12 hours. Next, the dried product was calcined in air at 400°C for 3 hours to obtain a spindle-shaped CeO2 catalyst carrier.

[0062] <Carrier 5: Cube-Shaped Ceria Catalyst Carrier and Lanthanum Oxide Composite Oxide Catalyst Carrier>

[0063] A solution prepared by adding 19.2 g of NaOH (97%, Daejung) to 50 ml of deionized water was added dropwise to a solution prepared by dissolving 1.73 g of Ce(NO3)3·6H2O (Sigma, 99%) and 0.87 g of La(NO3)3·6H2O (Sigma, 99%) in 30 ml of distilled water. Next, the solutions were mixed in a 100 ml polytetrafluoroethylene bottle and stirred continuously for 30 minutes. Finally, the polytetrafluoroethylene bottle was completely sealed and heated at 180°C for 12 hours in a stainless steel container autoclave. Next, the resulting precipitate was collected and washed several times with deionized water and ethanol, and then dried in an oven at 80°C for 24 hours, thereby producing a composite oxide, namely La(NO3)3·6H2O, which was in the shape of a cube and had a molar ratio of La to Ce of 0.33:0.67. 0.33 Ce 0.67 O2-cube.

[0064] <Carrier 6: Sphere-shaped ceria catalyst carrier>

[0065] 3 ml of acetic acid (Junsei, 99.7%) and ethylene glycol (Sigma, 99.8%) were added dropwise to a solution of 2.6 g of Ce(NO3)3·6H2O (Sigma, 99%) dissolved in 3 ml of deionized water. Next, the solution was mixed in a 100 ml polytetrafluoroethylene bottle and stirred continuously for 30 minutes. Finally, the polytetrafluoroethylene bottle was completely sealed and heated at 180°C for 3.5 hours in a stainless steel container autoclave. Next, the generated precipitate was collected and washed several times with deionized water and ethanol, then dried in an oven at 80°C for 12 hours, and then calcined at 500°C for 4 hours to obtain a spherical CeO2 catalyst carrier.

[0066] <Carrier 7: Rod-shaped ceria catalyst carrier>

[0067] 28.7 g of NaOH (Daejung, 97%) and 2.6 g of Ce(NO3)3·6H2O (Sigma, 99%) (OH - / Ce 3 +=120 molar ratio) were dissolved in 50ml and 30ml of deionized water respectively. Next, the two solutions were mixed in a 100ml polytetrafluoroethylene bottle and stirred continuously for 30 minutes. Finally, the polytetrafluoroethylene bottle was completely sealed and heated at 100°C for 24 hours in a stainless steel container autoclave. Next, the generated precipitate was collected and washed several times with deionized water and ethanol, then dried in an oven at 60°C for 24 hours, and then sintered at 500°C for 4 hours to obtain a rod-shaped CeO2 catalyst carrier.

[0068] <Carrier 8: Polycrystalline Ceria Catalyst Carrier>

[0069] 1.0 M NH4OH was added dropwise at a rate of 60 ml / h to a solution of 7.57 g of Ce(NO3)3·6H2O (Sigma, 99%) dissolved in 100 ml of deionized water until pH reached about 9. The solution was then stirred for 24 hours. The resulting precipitate was then collected and washed several times with deionized water and ethanol, dried in a vacuum oven at 110°C for 12 hours, and then calcined at 500°C for 4 hours to obtain a polycrystalline CeO2 catalyst carrier.

[0070] <Catalyst 1>

[0071] A ruthenium catalyst was produced by a deposition-precipitation (DP) method using the catalyst carrier of carrier 1. First, 1.0 g of the catalyst carrier of carrier 1 was suspended in 50 ml of deionized water, and then 0.04 g of RuCl3·xH2O (Sigma, 99.98%) was added to the suspension. The pH of the suspension was adjusted to 9.0 using a 0.5 M solution of NH4OH [0.5 L of a final solution was produced by diluting 16.3 ml of NH4OH (Samchun, 28-30%) in deionized water], and the resulting suspension was stirred at 400 rpm at room temperature and aged for 12 hours. Next, the resulting precipitate was filtered and separated, washed multiple times with deionized water and ethanol, and then dried at 110°C for 12 hours, thereby producing a catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium. The produced catalyst was labeled Ru / CeO2-cube (15).

[0072] <Catalyst 2>

[0073] A catalyst for ammonia decomposition reaction was manufactured in the same manner as catalyst 1, wherein the catalyst carrier of catalyst 1 was replaced with carrier 2, thereby manufacturing a catalyst for ammonia decomposition reaction loaded with 2 wt % of ruthenium. The manufactured catalyst was labeled Ru / CeO2-cube (10).

[0074] <Catalyst 3>

[0075] A catalyst for ammonia decomposition reaction was manufactured in the same manner as catalyst 1, wherein the catalyst carrier of catalyst 1 was replaced by carrier 3, thereby manufacturing a catalyst for ammonia decomposition reaction loaded with 2 wt % of ruthenium. The manufactured catalyst was labeled Ru / CeO2-cube (20).

[0076] <Catalyst 4>

[0077] A catalyst for ammonia decomposition reaction was prepared in the same manner as catalyst 1, wherein the catalyst carrier of catalyst 1 was replaced by carrier 5, thereby preparing a catalyst for ammonia decomposition reaction loaded with 2 wt% of ruthenium. The prepared catalyst is labeled Ru / La 0.33 Ce 0.67 O2-cube.

[0078] <Catalyst 5>

[0079] A catalyst for ammonia decomposition reaction was manufactured in the same manner as catalyst 1, wherein the catalyst carrier of catalyst 1 was replaced by carrier 4, thereby manufacturing a catalyst for ammonia decomposition reaction loaded with 2 wt % of ruthenium. The manufactured catalyst was labeled Ru / CeO2-spindle.

[0080] <Catalyst 6>

[0081] A catalyst for ammonia decomposition reaction was manufactured in the same manner as catalyst 1, wherein the catalyst carrier of catalyst 1 was replaced with carrier 6, thereby manufacturing a catalyst for ammonia decomposition reaction loaded with 2 wt % of ruthenium. The manufactured catalyst was labeled Ru / CeO2-sphere.

[0082] <Catalyst 7>

[0083] A catalyst for ammonia decomposition reaction was manufactured in the same manner as catalyst 1, wherein the catalyst carrier of catalyst 1 was replaced with carrier 7, thereby manufacturing a catalyst for ammonia decomposition reaction loaded with 2 wt % of ruthenium. The manufactured catalyst was labeled Ru / CeO2-rod.

[0084] <Catalyst 8>

[0085] A catalyst for ammonia decomposition reaction was manufactured in the same manner as catalyst 1, wherein the catalyst carrier of catalyst 1 was replaced with carrier 8, thereby manufacturing a catalyst for ammonia decomposition reaction loaded with 2 wt % of ruthenium. The manufactured catalyst was labeled Ru / CeO2-polycrystal.

[0086] <Catalyst 9>

[0087] A catalyst for ammonia decomposition reaction was prepared in the same manner as catalyst 1, wherein Al2O3 (Sigma, gamma phase) was used to replace the catalyst carrier of catalyst 1, thereby preparing a catalyst for ammonia decomposition reaction loaded with 2 wt% of ruthenium. The prepared catalyst was labeled Ru / Al2O3.

[0088] <Catalyst 10>

[0089] A catalyst for ammonia decomposition reaction was prepared in the same manner as Catalyst 1, except that MgO (Sigma) was used instead of the catalyst carrier of Catalyst 1 to prepare a catalyst for ammonia decomposition reaction carrying 2 wt % of ruthenium. The prepared catalyst was labeled Ru / MgO.

[0090] <Catalyst 11>

[0091] A ruthenium catalyst was produced by wet-impregnation (WI) using carrier 1. First, 1.0 g of the catalyst carrier of carrier 1 was suspended in 30 ml of deionized water, and after stirring for 30 minutes, 1.25 mL of Ru(NO)(NO3) was added. x (OH) y (Sigma, x+y=3, Ru 1.5%) and 4.95 ml of 0.04 M CsNO3 were added to the suspension at the same time, followed by additional stirring for 30 minutes. The stirred liquid was aged for 4 hours while rotating at 150 rpm at 60°C and 72 mbar using a rotary evaporator. Next, the resulting precipitate was dried at 110°C for 12 hours to produce a catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium and 2.6 wt% cesium. The produced catalyst was labeled Cs1Ru1 / CeO2-Cube.

[0092] <Catalyst 12>

[0093] The catalyst was prepared in the same manner as catalyst 11, and 4.95 ml of KNO3 was added to replace 4.95 ml of 0.04 M CsNO3 as a catalyst enhancer precursor, thereby preparing a catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium and 0.8 wt% potassium (K:Ru molar ratio = 1.0). The prepared catalyst was labeled K1Ru1 / CeO2-Cube.

[0094] <Catalyst 13>

[0095] The catalyst was prepared in the same manner as catalyst 11, and 4.95 ml of Ba(NO3)2 was added to replace 4.95 ml of 0.04 M CsNO3 as a catalyst enhancer precursor, thereby preparing a catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium and 2.6 wt% barium (Ba:Ru molar ratio = 1.0). The prepared catalyst was labeled Ba1Ru1 / CeO2-Cube.

[0096] <Catalyst 14>

[0097] The catalyst was prepared in the same manner as catalyst 11, and 4.95 ml of NaNO3 was added to replace 4.95 ml of 0.04 M CsNO3 as a catalyst enhancer precursor, thereby preparing a catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium and 0.4 wt% sodium (Na:Ru molar ratio = 1.0). The prepared catalyst was labeled Na1Ru1 / CeO2-Cube.

[0098] <Catalyst 15>

[0099] A catalyst was prepared in the same manner as catalyst 11, and 4.95 ml of Ca(NO3)2·4H2O was added to replace 4.95 ml of 0.04 M CsNO3 as a catalyst enhancer precursor, thereby producing a catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium and 0.8 wt% calcium (Ca:Ru molar ratio = 1.0). The produced catalyst was labeled Ca1Ru1 / CeO2-Cube.

[0100] <Catalyst 16>

[0101] A catalyst for ammonia decomposition reaction loaded with 2 wt % ruthenium and 2.6 wt % cesium was produced by the same method as catalyst 11, except that carrier 4 was used instead of carrier 1. The produced catalyst was labeled Cs1Ru1 / CeO2-spindle.

[0102] <Catalyst 17>

[0103] A catalyst for ammonia decomposition reaction loaded with 2 wt % ruthenium and 0.8 wt % calcium was produced by the same method as catalyst 11, except that the catalyst carrier was replaced by carrier 8. The produced catalyst was labeled as Ca1Ru1 / CeO2-polycrystal.

[0104] <Catalyst 18>

[0105] A catalyst for ammonia decomposition reaction loaded with 2 wt % ruthenium and 0.8 wt % calcium was produced by the same method as catalyst 11, except that the catalyst carrier was replaced by carrier 6. The produced catalyst was labeled as Ca1Ru1 / CeO2-sphere.

[0106] <Catalyst 19>

[0107] A catalyst for ammonia decomposition reaction carrying 2 wt % of ruthenium and 0.8 wt % of calcium was produced by the same method as catalyst 11, except that the catalyst carrier was replaced by carrier 7. The produced catalyst was labeled Ca1Ru1 / CeO2-rod.

[0108] <Catalyst 20>

[0109] The catalyst was prepared in the same manner as catalyst 11, and 2.47 ml of 0.04 M CsNO3 was used instead of 4.95 ml of 0.04 M CsNO3 to prepare a catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium and 1.3 wt% cesium. The prepared catalyst was labeled as Cs 0.5 Ru1 / CeO2-Cube.

[0110] <Catalyst 21>

[0111] A catalyst for ammonia decomposition reaction loaded with 2 wt% ruthenium and 5.2 wt% cesium was prepared by the same method as catalyst 11, and 9.9 ml of 0.04 M CsNO3 was used instead of 4.95 ml of 0.04 M CsNO3. The prepared catalyst was labeled Cs2Ru1 / CeO2-Cube.

[0112] <Test Example 1: Measurement of shape and physical properties of catalyst carrier>

[0113] The shapes and physical properties of catalysts 1, 4, 5 and catalysts 6, 7, and 8 were measured using a transmission electron microscope (TEM) measuring device (Titan G2 60-300S, FEI Company, USA), a specific surface area (BET) measuring device (TriStar II 3020, Micromeritics Company, USA), and a CO pulse chemisorption measuring device (ASAP 2020, Micromeritics Company, USA). The results are shown in the figure. Figure 1 and Figure 2 And as shown in Table 1.

[0114] In the SBET measurement of the catalyst support, degassing was performed at 300°C for 5 hours, nitrogen physical adsorption was performed at -196°C, and the specific surface area was calculated using the BET model.

[0115] The dispersion of Ru as an active material was determined using the CO pulse chemisorption technique. First, a heat treatment was performed at 100°C for 30 minutes in a pure oxygen environment, followed by a 30-minute purge using helium. Next, a reduction treatment was performed at 500°C for 2 hours in a hydrogen environment, and then an adsorption-desorption test of helium (30 minutes)-oxygen (30 minutes)-helium (30 minutes)-carbon dioxide (30 minutes)-helium (30 minutes)-hydrogen (30 minutes)-helium (30 minutes) was performed at 35°C. Finally, CO was injected to make CO / Ru = 1, thereby calculating the CO adsorption amount and the Ru dispersion.

[0116] [Table 1]

[0117]

[0118] like Figure 1 as well as Figure 2 As shown, it can be confirmed that the catalyst carrier produced by the method of the present invention can be produced in a specific shape by controlling the shape of the particles.

[0119] Furthermore, as shown in Table 1, it can be confirmed that the specific surface area of ​​the catalyst support and the degree of dispersion of ruthenium vary depending on the shape of the catalyst support.

[0120] <Test Example 2: Determination of Ammonia Decomposition Reaction Results>

[0121] The catalysts produced were used to perform ammonia dehydrogenation reactions and the ammonia conversion rate was measured. The measurement was performed at 6,000 ml / g under normal pressure. cat.The ammonia decomposition energy was measured at an ammonia space velocity of 1.500 ℃ / h and reaction temperatures of 300°C, 350°C, 400°C, 450°C and 500°C, and the ammonia conversion rate was calculated according to the following formula 1. The results are shown in Table 2 and Figure 3 shown.

[0122] [Formula 1]

[0123] Ammonia conversion rate (%) = [(ammonia concentration at reactor inlet) - (ammonia concentration at reactor outlet) / (ammonia concentration at reactor inlet) + (ammonia concentration at reactor outlet)] × 100

[0124] Variation of catalyst activity according to carrier type, shape, and carrier particle size

[0125] Table 2 below shows the results of measuring the ammonia conversion rate by performing ammonia dehydrogenation reactions using catalysts 1 to 10, respectively.

[0126] [Table 2]

[0127]

[0128] As shown in Table 2, the catalyst for ammonia decomposition reaction according to the present invention exhibits a higher ammonia conversion rate than the comparative example.

[0129] Comparison of Catalyst 1 and Catalysts 9 and 10 shows that, compared with the case where the cerium oxide in the catalyst carrier is alumina or magnesium oxide, even when the same Ru is supported, a significantly better ammonia conversion rate can be achieved, and cerium oxide is a relatively excellent carrier of Ru for ammonia decomposition catalysts. In addition, when La is introduced as a carrier in addition to Ce to form a composite oxide of Ce and La as shown in Catalyst 4, the ammonia decomposition activity can be further greatly increased, indicating that the ammonia decomposition activity can be increased when a composite oxide with other metals is used instead of cerium oxide alone.

[0130] By comparing catalysts 1, 5 to 8, it can be found that even in the same cerium oxide support, different ammonia conversion rates will be exhibited depending on the shape of the catalyst support. At the ammonia decomposition temperature, the order of ammonia conversion rates at 400°C is Ru / CeO2-cube>Ru / CeO2-spindle>Ru / CeO2-polycrystal>Ru / CeO2-sphere>Ru / CeO2-rod, indicating that the shape of the cerium oxide support will have a significant impact on the ammonia decomposition activity.

[0131] In addition, by comparing catalysts 1 to 3, it can be found that the ammonia decomposition activity also changes according to the particle size of cerium oxide. When the particle shape of cerium oxide is cube, the highest activity is shown when the particle size is about 15nm, followed by 20nm and 10nm.

[0132] Changes in catalyst activity according to the type and content of catalyst enhancer

[0133] Table 3 below shows the results of tests conducted while changing the catalyst enhancer in order to observe changes in activity in the ammonia decomposition reaction depending on the type of the catalyst enhancer.

[0134] [Table 3]

[0135]

[0136] In the ammonia decomposition catalyst using Ru, the activity is reduced when Ba, Na and Ca are introduced into the catalyst system, but the ammonia decomposition activity can be further improved when Cs and K are introduced compared with the case of using Ru alone, and the improvement effect of Cs is particularly significant. Therefore, the activity of the ammonia decomposition catalyst can be greatly improved by using Cs or the like as a catalyst enhancer. In addition, the effect of different contents of the catalyst enhancer is as follows Figure 3 As shown. The ammonia conversion rate also changes with the change in the content of the catalyst enhancer (catalysts 11, 20, and 21). Compared with catalyst 20, in which the molar ratio of Cs to Ru is 0.5, catalyst 11, which is 1.0 times, has a significantly improved ammonia conversion rate in all temperature ranges, while in catalyst 21, in which the molar ratio of Cs to Ru is 2.0, which further increases the Cs content, the ammonia conversion rate tends to decrease. This experiment confirmed that the best performance can be achieved when the molar ratio of the catalyst enhancer content to Ru is 1.0.

[0137] Activity variation of catalysts containing enhancers according to support shape

[0138] Table 4 below shows the effect of the shape of the cerium oxide support in the Ru catalyst containing Cs as a reinforcing agent.

[0139] [Table 4]

[0140]

[0141] In Table 4, the Ru catalyst system containing Cs as a reinforcing agent also shows differences in the activity of the ammonia decomposition catalyst according to the shape of the carrier, and the order of ammonia conversion at 400°C is Ru / CeO2-cube>Ru / CeO2-spindle>Ru / CeO2-polycrystal>Ru / CeO2-sphere>Ru / CeO2-rod, showing the same order as Table 2 without a reinforcing agent. It can be inferred that the effect of the reinforcing agent is independent of the shape of the carrier.

[0142] <Test Example 3: Measurement of long-term stability of catalyst>

[0143] The long-term stability of the catalysts was evaluated by performing a 100-hour ammonia dehydrogenation reaction using Catalyst 1 and Catalyst 8, respectively. The measurement was performed at 54,000 ml / g under normal pressure. cat. The measurement was carried out for 100 hours under the conditions of ammonia space velocity of 1 / h and reaction temperature of 500°C. The results showed that the ammonia conversion rate was as follows: Figure 4 shown.

[0144] pass Figure 4 It was confirmed that Catalyst 1 can stably maintain the catalytic activity at a higher conversion rate than Catalyst 8 over a reaction period of 100 hours or more.

[0145] <Test Example 4: Hydrogen-Programmed Temperature Reduction (H2-TPR) Analysis of Catalyst>

[0146] Hydrogen-programmed temperature reduction (H2-TPR) analysis was performed on catalysts 1, 7, 8, 9, 10, 11, 17, and 19. During the H2-TPR analysis, 0.05 g of the catalyst was heated to 110°C in an inert gas environment and then cooled to 35°C. Next, the temperature was raised to 1,000°C while supplying 10% H2 / Ar gas, and the heating rate was 10°C / min. As shown in the above H2-TPR analysis results, Figure 5 as well as Figure 6 A comparative diagram is shown in .

[0147] pass Figure 5 It can be confirmed that when Cs is added as a reinforcing agent, the temperature of the reduction peak of Ru shifts to the high temperature side and the area of ​​the reduction peak increases. This confirms that the addition of Cs can strengthen the interaction between Ru and the carrier (CeO2) and increase the relative content of Ru active material.

[0148] In addition, through Figure 6 It can be confirmed that when the molar ratio of Cs to Ru is 1.0, the temperature of the Ru reduction peak moves toward the highest temperature compared to the cases of 0.5 and 2.0, indicating that the strong interaction between Ru and the carrier and the higher relative content of Ru active material are important factors in improving the ammonia conversion rate.

[0149] This confirms that the catalyst for ammonia decomposition reaction according to the present invention has excellent catalytic activity in the ammonia decomposition reaction and can improve the ammonia conversion rate, and there is almost no problem of activity decline even under high temperature and long-term reaction conditions, indicating that its long-term stability is very excellent.

[0150] The present invention has been described in detail with reference to the embodiments in the above content, but it can also be implemented in different embodiments within the concept and scope of the present invention. Therefore, the scope of the present invention should be defined in the appended claims and their equivalents, and is not limited to the specific embodiments described in this specification.

Claims

1. A catalyst for ammonia decomposition reaction, characterized in that: The catalyst is a catalyst for ammonia decomposition reaction, comprising a catalyst carrier and a catalyst active material supported on the catalyst carrier. The catalyst active substance is ruthenium, The catalyst carrier is a cerium oxide having one or more shapes selected from the group consisting of a cube shape and a spindle shape. The size of the cube is 12nm to 18nm. The catalyst for ammonia decomposition reaction contains 0.1 wt % to 50 wt % of a catalyst active material relative to the total weight of the catalyst for ammonia decomposition reaction.

2. The catalyst for ammonia decomposition reaction according to claim 1, characterized in that: The catalyst carrier is a metal oxide composite in which one or more metal oxides selected from lanthanum (La), yttrium (Y), praseodymium (Pr), neodymium (Nd), samarium (Sm) and gadolinium (Gd) are composited with cerium oxide.

3. The catalyst for ammonia decomposition reaction according to claim 2, characterized in that: In the metal oxide composite, the molar ratio of cerium to the metal other than cerium is 40:60 to 95:

5.

4. The catalyst for ammonia decomposition reaction according to claim 1, characterized in that The catalyst for ammonia decomposition reaction contains one or more catalyst enhancers selected from the group consisting of cesium and potassium.

5. The catalyst for ammonia decomposition reaction according to claim 4, characterized in that: The catalyst for ammonia decomposition reaction comprises 0.01 wt % to 25 wt % of a catalyst enhancer relative to the total weight of the catalyst for ammonia decomposition reaction.

6. A method for producing hydrogen from ammonia, comprising producing hydrogen from ammonia using the catalyst for ammonia decomposition reaction according to any one of claims 1 to 5.

7. The method for producing hydrogen from ammonia according to claim 6, characterized in that The ammonia decomposition reaction is performed in the range of 300°C to 500°C.