Polyvinyl acetal resin
By adjusting the water absorption and structural unit content of the polyvinyl acetal resin, the dispersion of the magnetic powder and the mechanical strength of the molded body are improved, and the problems of poor dispersion and low mechanical strength of the magnetic powder in the existing technology are solved and achieved. Molded body with high mechanical strength and excellent dispersion.
Patent Information
- Application Number
- CN202180057574.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-09-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-09-24
AI Technical Summary
When the existing polyvinyl acetal resin is used, the ferrite magnetic powder has poor dispersion, resulting in low mechanical strength of the molded body and prone to settling, making it difficult to meet processing requirements.
By adjusting the average unit area water absorption of the polyvinyl acetal resin molded film to 2 mg/cm2 or more and 50 mg/cm2 or less, combined with appropriate adjustments to the hydroxyl group amount, acetal group amount, and acetyl group amount, a specific measurement is used The method and process conditions improve the dispersibility of the magnetic powder and the mechanical strength of the formed body.
It achieves excellent dispersion and high mechanical strength of ferrite powder, improves the base material adhesion and processing performance of the formed body, and avoids the occurrence of defects in the formed body.
Smart Images

Figure BDA0004113472520000041 
Figure BDA0004113472520000171
Abstract
Description
Technical Field
[0001] The present invention relates to a polyvinyl acetal resin which has excellent dispersibility and can produce a molded body having high mechanical strength. Background Art
[0002] Polyvinyl acetal resin is excellent in toughness, film-forming properties, dispersibility of inorganic powders such as pigments and organic powders, adhesion to the coating surface, etc. Therefore, it is used in applications such as ceramic green sheets constituting multilayer ceramic capacitors, conductive pastes, inks, coatings, enamels for sintering, and phosphating primers.
[0003] Among them, multilayer ceramic capacitors are generally manufactured through the following steps.
[0004] First, a slurry composition is obtained by adding ceramic raw material powder to a binder resin such as polyvinyl butyral resin and uniformly mixing them. The obtained slurry composition is applied to the surface of a support body that has been subjected to a demolding treatment. After the volatile components such as the solvent are distilled off by heating it, it is peeled off from the support body to obtain a ceramic green sheet. Next, a conductive paste containing polyvinyl butyral resin as a binder resin is applied to the obtained ceramic green sheet by screen printing, etc., and the obtained materials are alternately overlapped and heated and pressed to produce a laminate. Furthermore, after a degreasing treatment, sintering is performed, and external electrodes are sintered on the end faces of the obtained ceramic sintered product. After the above-mentioned process, a laminated ceramic capacitor is obtained.
[0005] Regarding such a binder resin, Patent Document 1 discloses that metal corrosion of peripheral equipment can be prevented by using a polyvinyl acetal resin obtained by acetalizing the polyvinyl alcohol using acetic acid obtained by generating acetic acid from sodium acetate remaining in polyvinyl alcohol as a catalyst.
[0006] Patent Document 2 discloses that the flexibility and thermal fusion properties of the obtained sheet can be improved by using a polyvinyl acetal resin obtained by acetalizing a specific modified polyvinyl alcohol with acetaldehyde and butyraldehyde.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent No. 3043106
[0010] Patent Document 2: Japanese Patent No. 3110146 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, for example, the dispersibility of magnetic powders such as ferrites is poor. When the polyvinyl acetal resin described in Patent Documents 1 and 2 is used as a binder resin, the magnetic powder cannot be fully dispersed in the slurry composition, or sedimentation occurs over time, and there is room for improvement in dispersibility and dispersion stability. In addition, when such a slurry composition is used, the mechanical strength of the obtained sheet is low, and defects may sometimes occur when the formed sheet is processed.
[0013] An object of the present invention is to provide a polyvinyl acetal resin which has excellent dispersibility and can produce a molded body having high mechanical strength.
[0014] Means used to solve problems
[0015] The present invention relates to a polyvinyl acetal resin having an average water absorption per unit area of 2 mg / cm2 when formed into a film having a thickness of 10 μm 2 Above and 50mg / cm 2 the following.
[0016] Hereinafter, the present invention will be described in detail.
[0017] The inventors have conducted intensive research and found that by adjusting the average water absorption per unit area under specified conditions, the dispersibility of difficult-to-disperse materials such as magnetic powders can be improved, and a film with high mechanical strength can be produced, thereby completing the present invention. It should be noted that in the present invention, high substrate adhesion can be exhibited.
[0018] The polyvinyl acetal resin of the present invention has an average water absorption per unit area of 2 mg / cm when formed into a film with a thickness of 10 μm. 2 Above and 50mg / cm 2 By making the average water absorption per unit area within the above range, the dispersibility of the ferrite is excellent and the strength of the obtained sheet can be improved. The preferred lower limit of the average water absorption per unit area is 3 mg / cm 2 The preferred upper limit is 40 mg / cm 2 The more preferred upper limit is 30 mg / cm 2 .
[0019] The above average water absorption per unit area can be calculated by the method described later.
[0020] Specifically, the polyvinyl acetal resin of the present invention is formed into a film with a thickness of 10 μm, and after drying at 70°C for 3 hours, it is placed in an environment with a temperature of 20°C and a humidity of 55% for more than 1 hour, and the weight A of the film is measured. Next, it is formed so that the water vapor of warm water at a temperature of 50°C is exposed to the main surface of the dried film. Then, when water droplets are observed on the surface of the film, the exposure of the water vapor is stopped, and the weight B of the formed film is measured. The water absorption is calculated by subtracting the weight A from the weight B. The water absorption per unit area is calculated by dividing the water absorption by the exposed area. It should be noted that in this specification, the state in which water droplets are observed on the surface of the film is referred to as the saturated water vapor amount.
[0021] In the above-mentioned measurement conditions of the water absorption per unit area, the water absorption rate of the polyvinyl acetal resin of the present invention is preferably 0.2 mg / min or more and 4.2 mg / min or less. By making the above-mentioned water absorption rate within the above-mentioned range, a strong sheet strength can be obtained. A more preferred lower limit of the above-mentioned water absorption rate is 0.3 mg / min, and a more preferred upper limit is 4.0 mg / min.
[0022] It should be noted that the water absorption rate can be measured by the same method as the water absorption per unit area. Specifically, the time from the start of water vapor exposure to the time when the water vapor exposure is stopped is measured, and the value obtained by dividing the average unit area film weight by the exposure time is taken as the water absorption rate.
[0023] In the present invention, in addition to the saponification degree, average polymerization degree, and half-peak width of the hydroxyl group of the polyvinyl alcohol used as the raw material, the conditions for acetalization can be adjusted, thereby making it possible to produce a polyvinyl acetal resin whose average water absorption per unit area when formed into a film with a thickness of 10 μm is within a prescribed range. In addition, by adjusting the hydroxyl amount of the polyvinyl acetal resin, the half-peak width of the hydroxyl group quantitatively measured by IR measurement, the half-peak width of the hydroxyl group quantitatively measured by NMR measurement and IR measurement, etc., it is also possible to produce a polyvinyl acetal resin whose average water absorption per unit area when formed into a film with a thickness of 10 μm is within a prescribed range.
[0024] The polyvinyl acetal resin of the present invention preferably has at least a structural unit having a hydroxyl group represented by the following formula (1), a structural unit having an acetal group represented by the following formula (2), and a structural unit having an acetyl group represented by the following formula (3).
[0025] [Chemical formula 1]
[0026]
[0027] In the above formula (2), R 1It represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.
[0028] In the above formula (2), R 1 In the case of an alkyl group having 1 to 20 carbon atoms, examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, 2-ethylhexyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, and octadecyl. Among them, methyl and n-propyl are preferred.
[0029] In the polyvinyl acetal resin of the present invention, the content of the structural unit having a hydroxyl group represented by the above formula (1) (hereinafter also referred to as "hydroxyl amount") is preferably 35 mol% and the preferred upper limit is 85 mol%. By making the hydroxyl amount above the above lower limit, it is easy to adjust the water absorption per unit area to within a specified range. As a result, the slurry composition obtained using the polyvinyl acetal resin of the present invention has excellent dispersibility and dispersion stability. In addition, the mechanical strength and substrate adhesion of the obtained molded body are improved.
[0030] The above-mentioned hydroxyl amount can be obtained, for example, by 13 C-NMR determination.
[0031] The preferred lower limit of the half-peak width of the hydroxyl group quantitatively determined by IR measurement of the polyvinyl acetal resin of the present invention is 280 cm -1 , the more preferred lower limit is 290cm -1 The upper limit is preferably 420cm -1 , the more preferred upper limit is 400cm -1 By setting it within the above range, it is easy to adjust the water absorption per unit area to the specified range. As a result, the slurry composition obtained using the polyvinyl acetal resin of the present invention has excellent dispersibility and dispersion stability. In addition, the mechanical strength and substrate adhesion of the obtained molded body are improved.
[0032] The polyvinyl acetal resin preferably has a half-peak width in terms of mol% of the hydroxyl group quantitatively determined by NMR measurement and IR measurement of 0.01 mol% / cm -1 More than 0.30 mol% / cm -1 By setting the above range, a ceramic green sheet having high mechanical strength and being less likely to have poor appearance after cutting or dimensional changes after drying can be obtained. In addition, the half-peak width converted by mole % of the hydroxyl group is more preferably 0.05 mole % / cm -1 Above 0.290 mol% / cm -1 the following.
[0033] In addition, the above-mentioned IR measurement refers to the measurement of the absorption spectrum based on infrared absorption spectroscopy, and can be measured by, for example, an IR meter.
[0034] The mol% converted half peak width of the hydroxyl group can be calculated as follows: -1 The half-peak width of the hydroxyl group was measured from the peak width at 1 / 2 of the peak height appearing near the peak, and then the amount of hydroxyl groups was measured by NMR measurement and calculated by dividing the amount of hydroxyl groups by the half-peak width of the hydroxyl group.
[0035] In the polyvinyl acetal resin of the present invention, the content of the structural unit having an acetal group represented by the above formula (2) (hereinafter also referred to as "acetal group amount") preferably has a lower limit of 1 mol% and an upper limit of 50 mol%.
[0036] When the amount of the acetal groups is within the above range, the toughness of the resin can be improved.
[0037] A more preferred lower limit of the amount of acetal groups is 2 mol%, and a more preferred upper limit is 45 mol%.
[0038] In the present specification, as a method for calculating the amount of acetal groups, since the acetal groups of the polyvinyl acetal resin are obtained by acetalizing two hydroxyl groups, the amount of acetal groups is calculated by counting the two hydroxyl groups acetalized.
[0039] The amount of acetal groups can be measured by, for example, NMR.
[0040] R in the above formula (2) 1 Preferred is methyl or propyl.
[0041] In the polyvinyl acetal resin of the present invention, R 1 In the case of a methyl group, the amount of acetal groups (acetal group amount) is preferably 1 mol% or more and 50 mol% or less.
[0042] In the polyvinyl acetal resin of the present invention, R 1 In the case of a propyl group, the amount of acetal groups (butyral groups) is preferably 1 mol% or more and 10 mol% or less. By setting it within the above range, a high water absorption capacity can be obtained.
[0043] In the polyvinyl acetal resin of the present invention, the content of the structural unit having an acetyl group represented by the above formula (3) (hereinafter also referred to as "acetyl group amount") preferably has a lower limit of 1 mol% and an upper limit of 20 mol%.
[0044] When the amount of the acetyl group is within the above range, the toughness of the resin can be improved.
[0045] A more preferred lower limit of the amount of acetyl groups is 2 mol %, and a more preferred upper limit is 15 mol %.
[0046] The acetyl group amount can be measured by, for example, NMR.
[0047] The polyvinyl acetal resin of the present invention may include a structural unit having an acid-modified group.
[0048] Examples of the acid-modified group include a carboxyl group, a sulfonic acid group, a maleic acid group, a sulfinic acid group, a sulfenic acid group, a phosphoric acid group, a phosphonic acid group, an amino group, and salts thereof, etc. Among them, a carboxyl group is preferred.
[0049] By providing the modified polyvinyl acetal resin with a structural unit having the acid-modified group, compatibility with the epoxy resin can be improved, thereby achieving high mechanical strength.
[0050] The structural unit having the acid-modified group may have a structure in which the acid-modified group as a side chain is directly bonded to the carbon constituting the main chain, or may have a structure in which the acid-modified group is bonded to the carbon constituting the main chain via an alkylene group.
[0051] The structural unit with the above-mentioned acid-modified group can be a three-dimensional structure in which two acid-modified groups are bonded to the same carbon constituting the main chain, or a three-dimensional structure in which one acid-modified group is bonded to the carbon constituting the main chain. In addition, it can be a three-dimensional structure in which one acid-modified group is bonded to the adjacent carbon constituting the main chain, or a three-dimensional structure in which the acid-modified group is only bonded to one of the adjacent carbons constituting the main chain. Among them, it is preferred to have: a three-dimensional structure in which two acid-modified groups are bonded to the same carbon constituting the main chain, or a three-dimensional structure in which one acid-modified group is bonded to the adjacent carbon constituting the main chain. In addition, from the perspective of being able to increase steric hindrance and expand the mesh structure of the cured product obtained by combining with epoxy resin, as a result, it is preferred that two acid-modified groups are bonded to the same carbon constituting the main chain.
[0052] In addition, the structural unit having the above-mentioned acid-modified group may have an isotactic structure in which the acid-modified group is bonded to the carbon constituting the main chain in the same direction, or may have a syndiotactic structure in which the acid-modified group is bonded to the carbon constituting the main chain alternately on the opposite sides. In addition, it may have an atactic structure in which the acid-modified group is randomly bonded.
[0053] When the structural unit having the above-mentioned acid-modified group has a structure in which the acid-modified group is bonded to the carbon constituting the main chain via a hydrocarbylene group, the above-mentioned hydrocarbylene group is preferably a hydrocarbylene group having 1 to 10 carbon atoms, more preferably a hydrocarbylene group having 1 to 5 carbon atoms, and further preferably a hydrocarbylene group having 1 to 3 carbon atoms.
[0054] Examples of the hydrocarbylene group having 1 to 10 carbon atoms include a linear hydrocarbylene group, a branched hydrocarbylene group, and a cyclic hydrocarbylene group.
[0055] Examples of the straight-chain hydrocarbylene group include a methylene group, a vinylene group, a n-propylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a decamethylene group.
[0056] Examples of the branched hydrocarbylene group include methylmethylene, methylethylene, 1-methylpentylene, and 1,4-dimethylbutylene.
[0057] Examples of the cyclic hydrocarbylene group include a cyclopropylene group, a cyclobutylene group, and a cyclohexylene group.
[0058] Among them, a straight-chain hydrocarbylene group is preferred, a methylene group, a vinylene group, and a n-propylene group are more preferred, and a methylene group and a vinylene group are further preferred.
[0059] The preferred lower limit of the average degree of polymerization of the polyvinyl acetal resin of the present invention is 200, and the preferred upper limit is 5000. When the average degree of polymerization is within the above range, the mechanical strength of the obtained coating film can be sufficiently improved.
[0060] A more preferred lower limit of the average degree of polymerization is 300, and a more preferred upper limit is 4,000.
[0061] Examples of a method for producing the polyvinyl acetal resin of the present invention include a method of acetalizing a polyvinyl alcohol resin obtained by adding an acid or a base to saponify a polyvinyl acetate resin obtained by polymerizing a monomer such as vinyl acetate.
[0062] In the present invention, by using polyvinyl alcohol having a saponification degree, an average polymerization degree, and a half-peak width of a hydroxyl group within a specified range and performing acetalization, a polyvinyl alcohol acetal resin having an average water absorption per unit area within a specified range when formed into a film with a thickness of 10 μm can be produced. For example, the half-peak width of the hydroxyl group of the polyvinyl alcohol resin is preferably 340 cm -1 Over 380cm -1 the following.
[0063] The polyvinyl alcohol resin preferably has an average degree of polymerization of 200 to 5000, and a degree of saponification of 70 mol % to 99.9 mol %.
[0064] In particular, the polyvinyl acetal resin of the present invention is preferably an acetalized product of a polyvinyl alcohol resin having a saponification degree of 75 mol % or more.
[0065] The specific polyvinyl alcohol described above can be prepared, for example, by measuring the physical properties of a plurality of polyvinyl alcohols to select the polyvinyl alcohol; by referring to the physical properties of commercially available polyvinyl alcohols to select the polyvinyl alcohol; or by adjusting the physical property values and synthesizing the polyvinyl alcohol through a predetermined process.
[0066] The acetalization can be carried out using a known method, and is preferably carried out in an aqueous solvent, in a mixed solvent of water and an organic solvent compatible with water, or in an organic solvent.
[0067] As the organic solvent compatible with water, for example, an alcohol organic solvent can be used.
[0068] Examples of the organic solvent include alcohol organic solvents, aromatic organic solvents, aliphatic ester solvents, ketone solvents, lower alkane solvents, ether solvents, amide solvents, and amine solvents.
[0069] Examples of the alcohol-based organic solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol.
[0070] Examples of the aromatic organic solvent include xylene, toluene, ethylbenzene, and methyl benzoate.
[0071] Examples of the aliphatic ester solvent include methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, methyl acetoacetate, and ethyl acetoacetate.
[0072] Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methylcyclohexanone, benzophenone, and acetophenone.
[0073] Examples of the lower alkane solvent include hexane, pentane, octane, cyclohexane, and decane.
[0074] Examples of the ether solvent include diethyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and propylene glycol diethyl ether.
[0075] Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetanilide.
[0076] Examples of the amine solvent include ammonia, trimethylamine, triethylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, aniline, N-methylaniline, N,N-dimethylaniline, and pyridine.
[0077] The above solvents may be used alone or in combination of two or more. Among these solvents, ethanol, n-propanol, isopropanol, and tetrahydrofuran are particularly preferred from the viewpoint of solubility in the resin and ease of purification.
[0078] The above-mentioned acetalization is preferably carried out in the presence of an acid catalyst.
[0079] The acid catalyst is not particularly limited, and examples thereof include mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, carboxylic acids such as formic acid, acetic acid, and propionic acid, and sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, and p-toluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more compounds. Among them, hydrochloric acid, nitric acid, and sulfuric acid are preferred, and hydrochloric acid is particularly preferred.
[0080] As the aldehyde used in the acetalization, there can be mentioned aldehydes having a chain aliphatic group, a cyclic aliphatic group or an aromatic group having 1 to 10 carbon atoms. As these aldehydes, conventionally known aldehydes can be used. The aldehyde used in the acetalization reaction is not particularly limited, and examples thereof include aliphatic aldehydes, aromatic aldehydes, and the like.
[0081] Examples of the aliphatic aldehydes include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, n-hexanal, 2-ethylbutyraldehyde, 2-ethylhexanal, n-heptylaldehyde, n-octanal, octanal, n-nonanal, n-decanal, and valeraldehyde.
[0082] Examples of the aromatic aldehyde include benzaldehyde, cinnamaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, m-hydroxybenzaldehyde, phenylacetaldehyde, β-phenylpropionaldehyde and the like.
[0083] In addition, cyclic polymers such as paraldehyde and tetramethyl acetaldehyde can be used.
[0084] These aldehydes may be used alone or in combination of two or more. As aldehydes, formaldehyde, acetaldehyde, butyraldehyde, 2-ethylhexanal, n-nonanal, and paraldehyde are preferred, as they have excellent acetalization reactivity, can provide sufficient internal plasticizing effect to the generated resin, and can impart good flexibility as a result. In addition, formaldehyde, acetaldehyde, butyraldehyde, and paraldehyde are more preferred from the perspective of obtaining an adhesive composition having particularly excellent impact resistance and adhesion to metals.
[0085] The amount of the aldehyde added can be appropriately set according to the acetal group amount of the target polyvinyl acetal resin. In particular, when the amount is set to 60 to 95 mol %, preferably 65 to 90 mol %, relative to 100 mol % of polyvinyl alcohol, the acetalization reaction proceeds efficiently and unreacted aldehyde is easily removed, which is preferred.
[0086] The slurry composition can be prepared by mixing the polyvinyl acetal resin of the present invention with magnetic powder, a solvent, etc. The slurry composition containing the polyvinyl acetal resin of the present invention, magnetic powder, and a solvent is also one of the present invention.
[0087] The content of the polyvinyl acetal resin of the present invention in the slurry composition of the present invention has a preferred lower limit of 20% by weight, and a more preferred lower limit of 25% by weight, and a preferred upper limit of 65% by weight, and a more preferred upper limit of 60% by weight.
[0088] The slurry composition of the present invention contains magnetic powder.
[0089] Examples of the magnetic powder include metal particles, metal oxide particles, and metal nitride particles.
[0090] Examples of the metal particles used as the magnetic powder include metal particles containing iron, cobalt, nickel, and alloys containing these metals.
[0091] Examples of the alloy include Fe—Ni, Fe—Co, Fe—Cr, Fe—Si, Fe—Al, Fe—Cr—Si, Fe—Cr—Al, Fe—Al—Si, Fe—Pt, and the like.
[0092] As the metal oxide, ferrite is preferred, and specifically, for example, MnFe 2 O 4 、CoFe 2 O 4 、NiFe 2 O 4 ,CuFe 2 O 4 、ZnFe 2 O 4 MgFe 2 O 4 , Fe 3 O 4 、MnFe 2 O 4 , Cu-Zn ferrite, Ni-Zn ferrite, Mn-Zn-ferrite, Ba ferrite, Ni-Cu-Zn ferrite, etc.
[0093] Examples of the metal nitride include Fe 2 N, Fe 3 N, Fe 4 N, Fe 16 N 2 、Sm 2 Fe 17 N 3 wait.
[0094] Examples of the shape of the above magnetic powder include spherical, ellipsoidal, disk, needle, rod, flat, tetrahedral structure, porous, and porous (porous in Japanese). Among them, spherical is preferred from the viewpoint of dispersibility and the like.
[0095] The above magnetic powder can be surface-treated with a silane coupling agent. By surface-treating the above magnetic powder with a silane coupling agent, even when a large amount of the above magnetic powder is compounded, aggregation between the magnetic powders can be suppressed.
[0096] Examples of the above silane coupling agent include amino silanes such as N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane; vinyl silanes such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane; methacryloyl silanes such as 3-methacryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropylmethyldimethoxysilane; mercapto silanes such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylethoxysilane; epoxy silanes such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane; ureido silanes such as 3-ureidopropyltriethoxysilane; isocyanate silanes such as 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane; alkyl silanes such as methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, isopropyl dimethoxysilane, isobutyltrimethoxysilane, cyclohexylmethyldimethoxysilane; phenyltrimethoxysilane, etc.
[0097] Examples of the method for surface-treating the above magnetic powder with a silane coupling agent include a wet method in which the treatment is carried out in a solution in which the above magnetic powder is dispersed; a dry method in which the above magnetic powder is directly treated in a powder state; an overall blending method in which the treatment is carried out in a resin composition obtained by dispersing the above magnetic powder in a resin, etc. Among them, the wet method is preferred from the viewpoint of suppressing aggregation of the magnetic powder.
[0098] The preferred lower limit of the average particle diameter of the above magnetic powder is 0.1 μm, and the preferred upper limit is 100 μm.
[0099] When the average particle size of the magnetic powder is within the above range, the adhesion to the substrate can be further improved.
[0100] A more preferred lower limit of the average particle size of the magnetic powder is 0.5 μm, and a more preferred upper limit is 70 μm.
[0101] The average particle size can be measured, for example, using a laser diffraction particle size distribution analyzer or the like.
[0102] The preferred lower limit of the content of the magnetic powder in the slurry composition of the present invention is 5% by weight, and a more preferred lower limit is 10% by weight. The preferred upper limit is 40% by weight, and a more preferred upper limit is 35% by weight.
[0103] As the solvent, water or an organic solvent compatible with water as described above can be used.
[0104] Examples of the organic solvent compatible with water include alcohols.
[0105] The slurry composition of the present invention may contain a resin other than the polyvinyl acetal resin, such as an acrylic resin and ethyl cellulose, within a range not impairing the effects of the present invention.
[0106] Furthermore, a plasticizer, a lubricant, an antistatic agent, and the like may be added to the slurry composition of the present invention within a range not impairing the effects of the present invention.
[0107] Effects of the Invention
[0108] According to the present invention, there can be provided a polyvinyl acetal resin which has excellent dispersibility and can produce a molded body having high mechanical strength. DETAILED DESCRIPTION
[0109] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0110] (Example 1)
[0111] (Production of polyvinyl acetal resin)
[0112] Polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half peak width of hydroxyl group 350 cm -1 )500g was added to 2500g of pure water and stirred at 90°C for about 2 hours to dissolve it. The solution was cooled to 40°C, 10g of hydrochloric acid with a concentration of 35% by weight was added thereto, the liquid temperature was lowered to 5°C, 75g of acetaldehyde was added, and the acetalization reaction was carried out while maintaining the temperature. Then, the liquid temperature was maintained at 65°C for 5 hours to terminate the reaction, and 40g of sodium hydroxide aqueous solution was added to carry out a neutralization reaction, thereby obtaining a polyvinyl acetal resin.
[0113] The obtained polyvinyl acetal resin was prepared using 13 The amount of acetal groups (the amount of acetal groups and the amount of butyral groups), the amount of hydroxyl groups, and the amount of acetyl groups were measured by C-NMR (nuclear magnetic resonance spectroscopy).
[0114] The obtained polyvinyl acetal resin was subjected to IR measurement using HORIBA FT-720 (manufactured by Horiba, Ltd.) to determine the half peak width of the hydroxyl group. The results are shown in Table 1.
[0115] Further, after measuring the half peak width of the hydroxyl group, the 13 The hydroxyl group amount measured by C-NMR measurement was divided by the half peak width of the hydroxyl group to calculate the half peak width in terms of mol % of the hydroxyl group.
[0116] (Example 2)
[0117] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half-peak width of hydroxyl group 345 cm) was used. -1 ), except for this, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, and the results of the acetal group amount (acetal group amount, butyral group amount), hydroxyl group amount, acetyl group amount, half-peak width of hydroxyl group, and half-peak width converted by mole % of hydroxyl group are shown in Table 1.
[0118] (Example 3)
[0119] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half-peak width of hydroxyl group 345 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 7.0 g, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, the amount of acetal groups (acetal groups, butyral groups), the amount of hydroxyl groups, the amount of acetyl groups, the half-peak width of the hydroxyl groups, and the half-peak width converted by mole % of the hydroxyl groups are shown in Table 1.
[0120] (Example 4)
[0121] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half peak width of hydroxyl group 380 cm) was used. -1 ), and 15.0 g of butyraldehyde was used instead of acetaldehyde, and a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1 are as shown in Table 1 for the acetal group amount (acetal group amount, butyral group amount), hydroxyl group amount, acetyl group amount, half-peak width of hydroxyl group, and half-peak width converted by mole % of hydroxyl group.
[0122] (Example 5)
[0123] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half-peak width of hydroxyl group 370 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 110 g, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, the amount of acetal groups (acetal groups, butyral groups), the amount of hydroxyl groups, the amount of acetyl groups, the half-peak width of the hydroxyl groups, and the half-peak width converted by mole % of the hydroxyl groups are shown in Table 1.
[0124] (Example 6)
[0125] A polyvinyl alcohol resin (saponification degree 90 mol%, average polymerization degree 600, half-peak width of hydroxyl group 335 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 7.0 g, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, the amount of acetal groups (acetal groups, butyral groups), the amount of hydroxyl groups, the amount of acetyl groups, the half-peak width of the hydroxyl groups, and the half-peak width converted by mole % of the hydroxyl groups are shown in Table 1.
[0126] (Example 7)
[0127] A polyvinyl alcohol resin (saponification degree 90 mol%, average polymerization degree 4500, half-peak width of hydroxyl group 345 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 75 g, and a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, and the results of the acetal group amount (acetal group amount, butyral group amount), hydroxyl group amount, acetyl group amount, half-peak width of hydroxyl group, and half-peak width converted by mole % of hydroxyl group are shown in Table 1.
[0128] (Example 8)
[0129] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half peak width of hydroxyl group 345 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 115 g, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, the amount of acetal groups (acetal groups, butyral groups), the amount of hydroxyl groups, the amount of acetyl groups, the half-peak width of the hydroxyl groups, and the half-peak width converted by mole % of the hydroxyl groups are shown in Table 1.
[0130] (Example 9)
[0131] A polyvinyl alcohol resin (saponification degree 95 mol%, average polymerization degree 600, half-peak width of hydroxyl group 345 cm) was used. -1), and the amount of acetaldehyde added was changed to 110 g, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, the amount of acetal groups (acetal groups, butyral groups), the amount of hydroxyl groups, the amount of acetyl groups, the half-peak width of the hydroxyl groups, and the half-peak width converted by mole % of the hydroxyl groups are shown in Table 1.
[0132] (Example 10)
[0133] A polyvinyl alcohol resin (saponification degree 82 mol%, average polymerization degree 600, half-peak width of hydroxyl group 345 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 60 g, and a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, and the results of the acetal group amount (acetal group amount, butyral group amount), hydroxyl group amount, acetyl group amount, half-peak width of hydroxyl group, and half-peak width converted by mole % of hydroxyl group are shown in Table 1.
[0134] (Comparative Example 1)
[0135] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half-peak width of hydroxyl group 335 cm) was used. -1 ), except for this, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, and the results of the acetal group amount (acetal group amount, butyral group amount), hydroxyl group amount, acetyl group amount, half-peak width of hydroxyl group, and half-peak width converted by mole % of hydroxyl group are shown in Table 1.
[0136] (Comparative Example 2)
[0137] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half-peak width of hydroxyl group 335 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 140 g, and a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, and the results of the acetal group amount (acetal group amount, butyral group amount), hydroxyl group amount, acetyl group amount, half-peak width of hydroxyl group, and half-peak width converted by mole % of hydroxyl group are shown in Table 1.
[0138] (Comparative Example 3)
[0139] A polyvinyl alcohol resin (saponification degree 88 mol%, average polymerization degree 600, half-peak width of hydroxyl group 335 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 5 g, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, the amount of acetal groups (acetal groups, butyral groups), the amount of hydroxyl groups, the amount of acetyl groups, the half-peak width of the hydroxyl groups, and the half-peak width converted by mole % of the hydroxyl groups are shown in Table 1.
[0140] (Comparative Example 4)
[0141] A polyvinyl alcohol resin (saponification degree 92 mol%, average polymerization degree 600, half-peak width of hydroxyl group 345 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 6 g, a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, the amount of acetal groups (acetal groups, butyral groups), the amount of hydroxyl groups, the amount of acetyl groups, the half-peak width of the hydroxyl groups, and the half-peak width converted by mole % of the hydroxyl groups are shown in Table 1.
[0142] (Comparative Example 5)
[0143] A polyvinyl alcohol resin (saponification degree 90 mol%, average polymerization degree 600, half peak width of hydroxyl group 470 cm) was used. -1 ), and the amount of acetaldehyde added was changed to 75 g, and a polyvinyl acetal resin was obtained in the same manner as in Example 1. The results of the measurements performed in the same manner as in Example 1, and the results of the acetal group amount (acetal group amount, butyral group amount), hydroxyl group amount, acetyl group amount, half-peak width of hydroxyl group, and half-peak width converted by mole % of hydroxyl group are shown in Table 1.
[0144] <Evaluation>
[0145] The polyvinyl acetal resins obtained in Examples and Comparative Examples were evaluated as follows.
[0146] (1) Determination of water absorption per unit area and water absorption rate
[0147] The polyvinyl acetal resins obtained in the examples and comparative examples were formed into films with a thickness of 10 μm by a doctor blade method, dried at 70° C. for 3 hours, and then placed in an environment of 20° C. and 55% humidity for more than 1 hour to measure the weight A of the films.
[0148] Next, water vapor of warm water at a temperature of 50°C was exposed to the main surface of the above-mentioned film. Then, when water droplets were observed on the surface of the above-mentioned film, the exposure was stopped and the weight B of the film was measured. The water absorption was calculated by subtracting the weight A from the weight B. In addition, the water absorption per unit area was calculated by dividing the above-mentioned water absorption by the exposed area.
[0149] In the examples and comparative examples of this specification, the exposed area is set to 40 cm 2 .
[0150] Furthermore, the time from the start of water vapor exposure to the time when the water vapor exposure was stopped (exposure time) was measured, and the value obtained by dividing the average film weight per unit area by the exposure time was calculated as the water absorption rate.
[0151] (2) Dispersion test (ferrite dispersion)
[0152] (Preparation of Slurry Composition)
[0153] With respect to 50 g of the obtained polyvinyl acetal resin, 21.4 g of ion exchange water, 28 g of ferrite as a magnetic powder, and 0.6 g of glycerol as a plasticizer were added, and stirred at 1200 rpm for 1.5 hours using a PRIMIX disperser, and then degassed at 1000 rpm for 30 minutes using a degassing Rentaro manufactured by Thinky Co., Ltd., to prepare a slurry composition. It should be noted that Ni-Cu-Zn ferrite was used as the ferrite.
[0154] (Particle size distribution measurement)
[0155] To the obtained slurry composition, 5 g of ethanol and 5 g of toluene were added and stirred to prepare an evaluation solution.
[0156] The obtained evaluation solution was subjected to particle size distribution measurement using a laser diffraction particle size distribution meter (manufactured by Horiba, Ltd., LA-910) to measure the D50 particle size of the magnetic powder. In addition, the D50 particle size after being placed at 23° C. for one week was also measured in the same manner. The rate of change of the D50 particle size was further calculated and evaluated according to the following criteria.
[0157] A: The change rate is less than 30%.
[0158] B: The change rate is 30% or more and less than 60%.
[0159] C: The change rate is 60% or more and less than 100%.
[0160] D: The change rate is 100% or more.
[0161] (3) Adhesion to substrate
[0162] (Production of resin sheets)
[0163] The obtained polyvinyl acetal resin was applied onto a release-treated PET film using a coater so as to have a thickness of 15 μm after drying, and then heated and dried at 70° C. for 120 minutes to prepare a resin sheet.
[0164] The obtained resin sheet was applied to various substrates (SPCC, PET, PC) so that the film thickness after drying would be 20 μm, and dried to prepare samples for measuring adhesion.
[0165] The adhesiveness of the obtained measurement sample was evaluated by the cross-cut test of JIS K 5400.
[0166] (4) Upper yield point stress, fracture point strain and fracture point stress
[0167] (sheet strength)
[0168] The upper yield stress (MPa), breaking strain (%) and breaking stress (MPa) of the obtained resin sheet were measured at a tensile speed of 20 mm / min using a tensile tester (manufactured by Shimadzu Corporation, AUTOGRAPH AGS-J) in accordance with JIS K 7113.
[0169]
[0170] Industrial Applicability
[0171] According to the present invention, there can be provided a polyvinyl acetal resin which has excellent dispersibility and can produce a molded body having high mechanical strength.
Claims
1. A polyvinyl acetal resin having an average water absorption per unit area of 2 mg / cm when formed into a film having a thickness of 10 μm 2 Above and 50mg / cm 2 the following, The polyvinyl acetal resin has a hydroxyl content of 35 mol% to 85 mol%, and a half-peak width of the hydroxyl group determined by IR measurement is 280 cm -1 ~420cm -1 , The acetal group content of the polyvinyl acetal resin is 1 mol% to 43 mol%.
2. The polyvinyl acetal resin according to claim 1, which has an average degree of polymerization of 200 to 5000. The polyvinyl acetal resin according to claim 1 or 2, which is an acetalized product of a polyvinyl alcohol resin having a saponification degree of 75 mol % or more. 4 . A slurry composition comprising the polyvinyl acetal resin according to claim 1 , a magnetic powder, and a solvent.