Hydrodesulfurization and denitrification catalyst gradation system and hydrodesulfurization and denitrification method
By modifying the alumina carrier and the catalyst gradation of specific metal elements, the pore volume and pore size distribution of the catalyst are optimized, which solves the problem of insufficient activity and stability of the existing diesel hydrodesulfurization and denitrification catalysts, and achieves efficient clean utilization of diesel. .
Patent Information
- Application Number
- CN202111274364.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The existing diesel hydrodesulfurization and denitrogenation catalyst gradation system has insufficient activity and stability, making it difficult to meet the demand for high-performance diesel clean utilization.
A catalyst gradation system composed of modified alumina carrier and specific metal elements (Group VIII and VIB metals) is used to optimize the pore volume and pore size distribution of the catalyst through the synergy of the catalyst with bimodal and unimodal pore distribution. Improve catalyst activity and stability.
It significantly improves the performance of diesel hydrodesulfurization and denitrification, enhances the stability and activity of the catalyst, and is suitable for diesel hydrogenation units in adiabatic reaction environments.
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrorefining, and in particular to a hydrodesulfurization and denitrification catalyst grading system and a hydrodesulfurization and denitrification method. Background Art
[0002] Under the background of green and low-carbon development, the demand for fossil fuels has been impacted, and the clean utilization of diesel has been challenged. On the one hand, environmental regulations require that the quality standards of clean diesel be gradually improved, and refineries must use better hydrogenation catalysts or technologies to remove sulfur and nitrogen impurities. On the other hand, the shrinking demand for diesel has put forward higher requirements for the clean utilization of diesel fractions, which requires the support of high-performance hydrogenation catalysts. Therefore, the development of high-performance desulfurization and denitrogenation hydrogenation catalysts and technologies is of great significance for the clean utilization of diesel. The diesel hydrogenation industrial unit is an adiabatic reaction unit. Due to the large exothermicity of the hydrogenation reaction, the radial temperature rise of the reactor is relatively high. Therefore, in different reaction zones, catalysts that match the reaction environment are selected, and a hydrogenation catalyst grading system is developed to better improve the hydrodesulfurization and denitrogenation performance of the diesel unit.
[0003] The patent application with application number 201811650785.1 discloses a method for deep hydrodenitrogenation of inferior high-nitrogen heavy distillate oil, in which a hydrogenation protection catalyst is loaded in the first reaction zone to remove impurities such as metals and colloids, a type I hydrodenitrogenation catalyst with high hydrogenation activity is loaded in the second reaction zone, and a type II hydrodenitrogenation catalyst with high hydrogenolysis activity is loaded in the third reaction zone. Through the grading of hydrogenation catalysts with different functions, the nitrides of condensed aromatic hydrocarbons replacing nitrogen heterocycles are deeply removed, providing low-nitrogen raw materials for hydrocracking and catalytic cracking catalysts.
[0004] The patent application with application number 201110192780.0 discloses that the reactor is divided into four reaction zones, which are respectively filled with the first type of catalyst, the mixture of the first type of catalyst and the second type of catalyst, the second type of catalyst and the first type of catalyst, wherein the first type of catalyst is Mo-Co catalyst and the second type of catalyst is W-Mo-Ni catalyst or W-Ni. The process treats high-sulfur, high-nitrogen low-quality diesel by grading different catalysts.
[0005] At present, the activity and stability of diesel hydrodesulfurization and denitrification catalyst systems are still insufficient. In order to enhance the comprehensive utilization of diesel, it is necessary to further promote the hydrodesulfurization and hydrodenitrogenation performance of diesel. Summary of the invention
[0006] The purpose of the present invention is to overcome the problem of insufficient activity and stability of the hydrodesulfurization and denitrification catalyst graded system in the prior art, and to provide a hydrodesulfurization and denitrification catalyst graded system and a hydrodesulfurization and denitrification method, wherein the graded system has good activity and stability and has excellent performance in hydrodesulfurization and denitrification.
[0007] In order to achieve the above-mentioned object, the first aspect of the present invention provides a hydrodesulfurization and denitrification catalyst grading system, the grading system comprising a first catalyst and a second catalyst arranged in sequence along a logistics direction;
[0008] The first catalyst comprises a metal element of Group VIII, a metal element of Group VIB and a modified alumina carrier, and has a pore volume of 0.15-0.5 cm 3 / g, with an average pore size of 6-15nm, wherein the pore size of the catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm;
[0009] The second catalyst comprises a modified alumina carrier and a metal element of Group VIII, a metal element of Group VIB and a phosphorus element supported on the modified alumina carrier, and has a pore volume of 0.3-0.55 cm 3 / g, with an average pore size of 7-15nm, wherein the pore size of the second catalyst presents a unimodal pore distribution in the range of 8-20nm;
[0010] The modified alumina supports in the first catalyst and the second catalyst each independently contain a weakly acidic component.
[0011] The second aspect of the present invention provides a method for hydrodesulfurization and denitrification, which comprises: reacting the distillate oil to be treated with the grading system described in the first aspect under hydrodesulfurization and denitrification conditions.
[0012] Through the above technical scheme, the first catalyst and the second catalyst having specific structures and compositions are coordinated and matched, which is particularly suitable for hydrodesulfurization and denitrification in the clean production of diesel, and has excellent industrial value. DETAILED DESCRIPTION
[0013] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0014] The first aspect of the present invention provides a hydrodesulfurization and denitrification catalyst grading system, the grading system comprising a first catalyst and a second catalyst arranged in sequence along a logistics direction;
[0015] The first catalyst comprises a metal element of Group VIII, a metal element of Group VIB and a modified alumina carrier, and has a pore volume of 0.15-0.5 cm 3 / g, with an average pore size of 6-15nm, wherein the pore size of the catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm;
[0016] The second catalyst comprises a modified alumina carrier and a metal element of Group VIII, a metal element of Group VIB and a phosphorus element supported on the modified alumina carrier, and has a pore volume of 0.3-0.55 cm 3 / g, with an average pore size of 7-15nm, wherein the pore size of the second catalyst presents a unimodal pore distribution in the range of 8-20nm;
[0017] The modified alumina supports in the first catalyst and the second catalyst each independently contain a weakly acidic component.
[0018] In the present invention, the pore volume, average pore diameter and pore distribution of the catalyst are measured after the catalyst is calcined at 400 degrees for 3 hours.
[0019] In the present invention, a first catalyst containing bimodal pores and a second catalyst containing unimodal pores are used for grading, so that sulfides and nitrides of different sizes are firstly removed well on the first catalyst, and then passed through the second catalyst under a high temperature environment, focusing on removing the remaining difficult-to-react sulfides and nitrides, so as to achieve the effect of giving full play to the advantages of their respective desulfurization and denitrification, so that the graded system has good desulfurization and denitrification effects, and is more suitable for the adiabatic reaction environment of diesel hydrodesulfurization and denitrification.
[0020] In the present invention, the specific surface area, pore volume, average pore diameter and pore distribution of the catalyst are measured by low temperature nitrogen adsorption method (BET) (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). Among them, the pore volume of 2-100 nm is calculated according to the results of BET.
[0021] In the present invention, unless otherwise specified, the 2-6nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 6nm, the 2-4nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 4nm, the 4-6nm pores refer to pores with a pore diameter greater than or equal to 4nm and less than 6nm, and the 8-20nm pores refer to pores with a pore diameter greater than or equal to 8nm and less than 20nm.
[0022] In the present invention, the pore size of the first catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm, which means that the pore size distribution of the catalyst has peaks in the pore size range of 2-6nm and 8-20nm. Generally, the carrier also has a certain number of pore size distributions in the range of 2-6nm, but this part of the pores of the carrier does not have a peak, and no bimodal pores are formed.
[0023] The modified alumina carriers of the first catalyst and the second catalyst described in the present invention each independently contain a weakly acidic component, and the modified alumina carriers used by the two may be the same or different, and the weakly acidic components contained may also be the same or different, preferably the same. The modified alumina carriers selected for the first catalyst and the second catalyst of the present invention contain at least a certain amount of acidic components, which can promote the dispersion of active components and promote the hydrogenation activity of the catalyst, and more effectively improve the performance of the catalyst in a limited space. The weakly acidic component can be added in any process of the preparation of the alumina carrier, such as adding it to the pseudo-boehmite powder, adding it during the carrier preparation process, or adding it after the alumina carrier is formed. According to the present invention, there is no specific limitation on the types of weakly acidic components in the first catalyst and the second catalyst. Preferably, the weakly acidic component is selected from at least one of B, P, Si, F and Ge elements; further preferably, the weakly acidic component is selected from at least one of B, P and Si elements.
[0024] In the present invention, there is no specific limitation on the content of the weak acid component, as long as it can meet the performance requirements of the catalyst. Preferably, in the modified alumina carrier, the content of the weak acid component is 0.5-10 wt %, more preferably 1.5-8 wt %, calculated as oxide.
[0025] In the present invention, the weakly acidic component is provided by a compound containing a weakly acidic component. In a preferred embodiment, in the modified alumina carrier, the content of B2O3 is not more than 5 weight%, or the content of P2O5 is not more than 6 weight%, or the content of SiO2 is not more than 10 weight%, or the content of F is not more than 5 weight%, or the content of GeO2 is not more than 6 weight%.
[0026] In a particularly preferred embodiment, the modified alumina carrier has a B2O3 content of 1.5-5% by weight, a P2O5 content of 2-6% by weight, a SiO2 content of 6-10% by weight, a F content of 1-3% by weight, or a GeO2 content of 2-4% by weight.
[0027] In the present invention, there is no specific limitation on the method for introducing the weakly acidic component, and conventional methods in the art are applicable to the present invention. For example, an impregnation method can be selected. In a preferred embodiment, the present invention adopts a co-impregnation method to introduce the weakly acidic component.
[0028] In the present invention, there is no particular restriction on the timing of introducing the weakly acidic component, and the weakly acidic component can be introduced during the preparation of the alumina support or after the preparation of the alumina support. Preferably, the following method can be adopted: the weakly acidic component is introduced after the preparation of the alumina support, and then calcined to obtain a modified alumina support.
[0029] In the present invention, when the weakly acidic component is introduced after the alumina carrier is prepared, the weakly acidic component is provided by a compound containing the weakly acidic component. Preferably, the compound containing the weakly acidic component is selected from at least one of boric acid, silica sol, phosphoric acid, hypophosphorous acid, ammonium phosphate, ammonium dihydrogen phosphate, ammonium fluoride, sodium germanate and germanium hydroxide.
[0030] In the present invention, the specific conditions for calcination can be selected in a wide range. Preferably, the calcination temperature is 500-800°C and the calcination time is 2-10 hours.
[0031] In the present invention, when the weakly acidic component is introduced during the preparation of the alumina carrier, preferably, the compound containing the weakly acidic component can be directly added in the form of a precursor.
[0032] There is no specific limitation on the preparation method of the alumina carrier in the present invention. Conventional preparation methods in the art are applicable to the present invention and will not be described in detail herein.
[0033] In the present invention, it is preferred to select alumina with specific physical properties as the carrier of modified alumina. Preferably, the water absorption rate of alumina in the modified alumina carrier is greater than 0.9 mL / g, and the specific surface area is greater than 250 m 2 / g, the average pore size is greater than 9nm, and further preferably, in the modified alumina carrier, the water absorption rate of alumina is 0.9-1.1mL / g, and the specific surface area is 250-360m 2 / g, the average pore size is 9-14nm, and the pore distribution is a single peak pore distribution. This preferred embodiment can give full play to the effect of the active metal in the smaller pores and the larger pores, improve the reaction efficiency of the catalyst for reaction substrates of different sizes, and achieve the purpose of fully utilizing the active metal.
[0034] In a preferred embodiment, in the alumina, the pore volume with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the modified alumina carrier, more preferably no more than 8%, and even more preferably 5-8%.
[0035] In a preferred embodiment, in the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4%, preferably no more than 3% of the total pore volume of the alumina.
[0036] The use of the above preferred modified alumina carrier is more conducive to the loading of active components and avoids the formation of agglomerated particles.
[0037] In a preferred embodiment, in the first catalyst, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 7-15% of the total pore volume of the catalyst, and more preferably 8-13%.
[0038] In a preferred embodiment, the first catalyst and the second catalyst each independently contain P2O5, where P2O5 refers to P2O5 other than the compound containing the P weakly acidic component introduced into the modified alumina carrier.
[0039] In the present invention, in order to better utilize the pores of the catalyst and give full play to the performance of the catalyst. Preferably, the first catalyst composition is (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the modified alumina carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the modified alumina carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of the modified alumina carrier P2O5, Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-1nm, preferably 0.4-0.85nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of the modified alumina support.
[0040] It is worth noting that ci here is the mass of P2O5 relative to 1 gram of the modified alumina carrier, and P2O5 refers to P2O5 other than the weakly acidic component P2O5 in the modified alumina carrier, that is, it does not include the weakly acidic component P2O5 in the modified alumina carrier.
[0041] In the present invention, ρMoO3, ρWO3, ρNiO, ρCoO, and ρP2O5 are 4.69 g / cm 3 , 7.16g / cm 3 、6.67g / cm 3 、6.45g / cm 3 and 2.39 g / cm 3 calculate.
[0042] In the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co and Ni, preferably Co and / or Ni.
[0043] In a preferred embodiment, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.
[0044] In the present invention, there is no particular limitation on the amount of P2O5 and the metal oxide of Group VIB. Preferably, the molar ratio of Zi / Xi in the first catalyst is 0.1-0.4, more preferably 0.1-0.35. The advantage of adopting this preferred embodiment is that the metal components can better exert the synergistic effect with each other, thereby optimizing the activity of the catalyst.
[0045] In the present invention, the second catalyst is also limited in composition. Preferably, the second catalyst composition is (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the modified alumina carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the modified alumina carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of the modified alumina carrier P2O5, Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.2-0.39nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of the modified alumina support.
[0046] In the present invention, the selection range of the types of the Group VIII metal elements and the Group VIB metal elements in the second catalyst is the same as that of the first catalyst, and will not be elaborated here.
[0047] In the present invention, there is no particular limitation on the amount of P2O5 and the Group VIB metal oxide in the second catalyst. Preferably, the molar ratio of Zi / Xi in the catalyst is 0.05-0.45:1, more preferably 0.2-0.38:1.
[0048] In the present invention, in order to improve the performance of the first catalyst and the second catalyst, the atomic concentration of the VIB group metal element in the first catalyst and the second catalyst is limited. Preferably, the atomic concentration of the VIB group metal element in the first catalyst on the surface of the modified alumina carrier is 4.5-14atom / nm 2 , preferably 5-12atom / nm 2 .
[0049] In a preferred embodiment, the atomic concentration of the VIB group metal element in the second catalyst on the surface of the modified alumina carrier is 2-5.5 atom / nm 2 , preferably 3-4.5atom / nm 2 .
[0050] In the present invention, the atomic concentration of the VIB group metal element in the first catalyst and the second catalyst on the surface of the modified alumina carrier refers to the average atomic concentration of the VIB group metal element on the surface of the modified alumina carrier, which is obtained by measuring the metal loading and the specific surface area of the carrier and then calculating. Specifically, it can be obtained by the following calculation: (ai / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of modified alumina carrier Xi, M Xi is the molecular weight of Xi, SA sup is the specific surface area of the carrier.
[0051] In a preferred embodiment, in order to further improve the performance of the first catalyst and the second catalyst, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the first catalyst is 0.1-0.4, preferably 0.2-0.3.
[0052] In a preferred embodiment, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the second catalyst is 0.2-0.38, preferably 0.2-0.3.
[0053] In the present invention, preferably, the first catalyst and the second catalyst further independently include an organic alcohol compound and / or a carboxylic acid compound. The types of the organic alcohol compound and / or the carboxylic acid compound in the first catalyst and the second catalyst may be the same or different, and the present invention has no particular limitation, but they are preferably the same.
[0054] In a preferred embodiment, in the first catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the metal element of Group VIII is 1-6, preferably 2-5.
[0055] In a preferred embodiment, in the second catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the metal element of Group VIII is 1-4, preferably 2-4.
[0056] The purpose of adopting this preferred embodiment is to ensure that the metal elements of Group VIII have a higher dispersibility, weaken the interaction between the modified alumina support and the metal, and promote the generation of more active phases.
[0057] In a preferred embodiment, the organic alcohol compound can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. In a particularly preferred embodiment, the organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane. In a more particularly preferred embodiment, the organic alcohol compound is selected from at least one of glycerol, propanol and ethylene glycol.
[0058] In a preferred embodiment, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, and is further preferably at least one of formic acid, citric acid and acetic acid.
[0059] In a particularly preferred embodiment, the first catalyst and the second catalyst each independently include one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.
[0060] According to the present invention, there is no specific restriction on the amount of the first catalyst and the second catalyst in the graded system. Preferably, the loading volume ratio of the first catalyst to the second catalyst is 1:4-4:1, preferably 1:3-3:1.
[0061] According to the present invention, there is no specific limitation on the size of the first catalyst and the second catalyst, as long as they can meet the use requirements. Preferably, the equivalent diameters of the first catalyst and the second catalyst are independently 0.5-1.8 mm, preferably 0.8-1.6 mm.
[0062] According to the present invention, there is no specific limitation on the shapes of the first catalyst and the second catalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the shapes of the first catalyst and the second catalyst are each independently cylindrical, clover, four-leaf clover, honeycomb or other irregular shapes, and more preferably butterfly-shaped.
[0063] According to the present invention, there is no specific limitation on the preparation methods of the first catalyst and the second catalyst. Preferably, the preparation methods of the first catalyst and the second catalyst each independently comprise: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound and / or a carboxylic acid compound into a modified alumina carrier by an impregnation method, and then drying.
[0064] In the present invention, the “optionally organic alcohol compounds and / or carboxylic acid compounds” means that organic alcohol compounds and / or carboxylic acid compounds may or may not be introduced into the modified alumina carrier. In the present invention, introduction is preferred.
[0065] In the present invention, the types of Group VIII metals, Group VIB metals, organic alcohol compounds, and carboxylic acid compounds have been described above and will not be described again here.
[0066] In a preferred embodiment, the Group VIB metal precursor includes, but is not limited to, one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate and tungsten oxide.
[0067] In a preferred embodiment, the Group VIII metal precursor includes, but is not limited to, one or more of cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0068] In a particularly preferred case, the Group VIB metal and Group VIII metal precursors include but are not limited to one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate, tungsten oxide, cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0069] In a preferred case, P2O5 is provided by a phosphorus-containing compound. Further preferably, the phosphorus-containing compound includes but is not limited to one or more of phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.
[0070] In a preferred embodiment, the amount of the Group VIII metal precursor, the Group VIB metal precursor, and the phosphorus-containing compound is such that the catalyst obtained satisfies the above (ai / ρ Xi +bi / ρ Yi+ci / ρ Zi ) / SA sup The value required.
[0071] According to the preparation method of the present invention, there is no specific limitation on the impregnation method, and conventional impregnation methods in the art are applicable to the present invention. For example, it can be one of co-impregnation, step-by-step impregnation, saturated impregnation and supersaturated impregnation. In a preferred embodiment, the present invention adopts a co-impregnation method to prepare the catalyst. In a more preferred embodiment, the impregnation method comprises: impregnating the modified alumina carrier with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound and / or a carboxylic acid compound.
[0072] In the present invention, there is no specific limitation on the order of adding the Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound, and optionally the organic alcohol compound and / or the carboxylic acid compound, as long as it is conducive to uniform mixing of the components. In a preferred embodiment, the Group VIII metal precursor, the Group VIB metal precursor and the organic alcohol compound and / or the carboxylic acid compound are added to an aqueous solution of the phosphorus-containing compound to prepare the impregnation solution. In the present invention, the order of adding the organic alcohol compound and / or the carboxylic acid compound, the phosphorus-containing compound and the metal precursor can also be interchanged.
[0073] According to the present invention, the prepared catalyst has the aforementioned structure and composition according to the physical properties of the modified alumina carrier and the amount of each material. The present invention has no particular limitation on this. In order to facilitate the understanding of the technical solution of the present invention, an exemplary description is now provided to reflect the preparation method of the first catalyst of the present invention. The method of the present invention includes but is not limited to this. For example, the first catalyst can be prepared by the following preparation method: (1) According to the surface concentration of the VIB group metal element and the specific surface area of the modified alumina carrier, the feeding amount of the VIB group metal precursor relative to each gram of the modified alumina carrier is determined; (2) According to the atomic ratio of the VIII group metal element to the total amount of the VIII group metal element and the VIB group metal element, the feeding amount of the VIII group metal precursor relative to each gram of the modified alumina carrier is determined; (3) According to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA supThe content of P2O5 is calculated based on the value of , and then the amount of phosphorus-containing compound per gram of carrier is determined; (4) the amount of organic alcohol compound and / or carboxylic acid compound is calculated based on the molar ratio of organic alcohol compound and / or carboxylic acid compound to Group VIII metal element; (5) according to the above-mentioned amounts of Group VIB metal precursor, Group VIII metal precursor, phosphorus-containing compound and organic alcohol compound and / or carboxylic acid compound, the modified alumina carrier is impregnated with the impregnation liquid by pore saturation impregnation method, and then dried. Specifically, a phosphorus-containing compound is first dissolved in water to obtain a phosphorus-containing aqueous solution, and then an organic alcohol compound and / or a carboxylic acid compound, a Group VIB metal precursor and a Group VIII metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is maintained to obtain an impregnation solution; (6) the water absorption rate of the modified alumina carrier is measured, and the liquid absorption rate of the modified alumina carrier is calculated according to the formula of water absorption rate of the modified alumina carrier-0.1; (7) according to the liquid absorption rate of the modified alumina carrier, the impregnation solution is diluted to a corresponding volume (liquid absorption rate of the modified alumina carrier×mass of the carrier), and the impregnation solution and a corresponding mass of the modified alumina carrier are evenly mixed and allowed to stand, and then dried to prepare a first catalyst.
[0074] In the present invention, the drying conditions have a wide range of selections. Preferably, the drying conditions include: a temperature of 80-200° C. and a time of 1-10 h.
[0075] According to the present invention, the preparation methods of the second catalyst and the first catalyst may be the same, which will not be described in detail herein.
[0076] The second aspect of the present invention provides a method for hydrodesulfurization and denitrification, which comprises: reacting the distillate oil to be treated with the grading system described in the first aspect under hydrodesulfurization and denitrification conditions.
[0077] In a preferred embodiment, before the graded system reaction is performed, the first catalyst and the second catalyst need to be vulcanized from an oxidized catalyst to a vulcanized catalyst. In the present invention, there is no specific limitation on the vulcanization method, and conventional vulcanization methods in the art are applicable to the present invention. Preferably, for example, it can be one of dry vulcanization and wet vulcanization. There is no particular limitation on the type of vulcanizing agent, and it can be selected according to conventional solutions in the art.
[0078] Preferably, the vulcanization conditions include: vulcanization temperature of 280-420°C, time of 10-48h, pressure of 0.1-15MPa, volume space velocity of 0.5-20h -1 , the volume ratio of hydrogen to oil is 100-2000:1, and the preferred heating rate is 5-60°C / hour.
[0079] The method for hydrodesulfurization and denitrogenation can be carried out in a hydrogenation device, in which the above-mentioned gradation system is provided. According to the present invention, the hydrogenation device can be selected from any conventional reactor, as long as the raw material can be contacted and reacted with the first catalyst and the second catalyst in sequence. For example, two reactors can be connected in series to form a first reaction zone and a second reaction zone, the first catalyst is loaded in the first reaction zone, the second catalyst is loaded in the second reaction zone, and the raw material flows through the first reactor and then passes into the second reactor for reaction. The reactor can also be divided into a first reaction zone and a second reaction zone arranged up and down, the first catalyst and the second catalyst are loaded in the two reaction zones respectively, and the raw material is injected into the reactor from top to bottom for reaction.
[0080] In a preferred embodiment, the distillate to be treated has a nitrogen content of 4000-15000 ppm and a nitrogen content of 200-3000 ppm.
[0081] In a preferred embodiment, the conditions for hydrodesulfurization and denitrification include: temperature of 300-420°C, pressure of 5-15 MPa, volume space velocity of 0.5-10 hours -1 , the volume ratio of hydrogen to oil is 250-2500:1.
[0082] According to the present invention, the first catalyst is loaded in the first reaction zone, the second catalyst is loaded in the second reaction zone, and the conditions of the first reaction zone include: temperature of 300-390°C, pressure of 5-15MPa, volume space velocity of 0.5-10h -1 , the hydrogen-to-oil volume ratio is 250-2000:1, and the conditions of the second reaction zone include: temperature of 360-420°C, pressure of 5-15MPa, volume space velocity of 0.5-10h -1 The volume ratio of hydrogen to oil is 250-2500:1. The above preferred implementation is beneficial for the first catalyst and the second catalyst to perform desulfurization and denitrification reactions respectively, and promotes the stability of the overall catalyst grading system.
[0083] The present invention will be described in detail below through examples. The performance of the catalyst system of the present invention is evaluated in the following manner: In the following examples, the hydrodesulfurization performance of the catalyst grading system is measured in a small evaluation device. The device is provided with two reactors connected in series, the first reactor is filled with the first catalyst of the present invention, and the second reactor is filled with the second catalyst of the present invention. The oxidized catalyst is directly converted into a sulfurized catalyst by a programmed temperature sulfurization method. The sulfurization conditions are: the sulfurization pressure is 6.4MPa, the sulfurized oil is kerosene containing 2% by weight of CS2, and the volume space velocity is 2h -1, the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then increase the temperature to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials to carry out the hydrodesulfurization and denitrification activity test. The reaction raw materials are distillate oil with a sulfur content of 10890ppm and a nitrogen content of 321ppm. The test conditions are: the pressure is 6.4MPa, and the total volume space velocity of the two reactors is 2h -1 , the volume ratio of hydrogen to oil is 300v / v. The properties of the product were analyzed after the reaction was stable for 2 days. In order to examine the stability of the catalyst, the mass fraction of sulfur in the reaction product was kept at 10ppm, the reaction temperature was adjusted every day, and the operation was continued for 5 days. The changes in the reaction temperature before and after 5 days were compared to measure the stability of the catalyst.
[0084] The composition of the catalyst is calculated based on the feed amount. The specific surface area of 2-100 nm, pore distribution, pore diameter, and pore volume in the catalyst and modified alumina carrier are determined by low-temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The mass fraction of sulfur and nitrogen in the product is analyzed using a sulfur-nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000).
[0085] Example 1
[0086] The preparation process and properties of the first catalyst are as follows:
[0087] A γ-alumina carrier was selected, and after the carrier was prepared, 2 wt% B2O3 was introduced by impregnation method to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 1.02 mL / g, and the specific surface area was 271 m 2 / g, the average pore size is 12.5nm, the pore volume with a pore size of 2-6nm accounts for 7.4% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0088] MoO3, basic nickel carbonate and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0089] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0090] The atomic concentration of Mo in the catalyst is 6.7atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.29, P2O5 / MoO3 molar ratio is 0.13, (ai / ρXi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbonyl group is 0.485 nm, and the molar ratio of glycerol to Ni is 2.
[0091] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 161m 2 / g, pore volume 0.36cm 3 / g, the average pore diameter is 8.9nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 10.5% of the total pore volume.
[0092] The preparation process and properties of the second catalyst are as follows:
[0093] A γ-alumina carrier was selected, and after the carrier was prepared, 2 wt% B2O3 was introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 1.02 mL / g, and the specific surface area was 271 m 2 / g, the average pore size is 12.5nm, the pore volume with a pore size of 2-6nm accounts for 7.4% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0094] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0095] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0096] The atomic concentration of Mo in the catalyst is 4.3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.33 nm, and the molar ratio of glycerol to Ni is 2.
[0097] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 188m 2 / g, pore volume 0.43cm 3 / g, the average pore size is 9.1nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0098] Performance test of catalyst grading system:
[0099] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 1:1. The reaction temperature of the first catalyst was 355°C and the reaction temperature of the second catalyst was 380°C. After the reaction test, the sulfur content in the product was 4.3ppm and the nitrogen content was 1.3ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.5°C after 5 days of reaction.
[0100] Example 2
[0101] The preparation process and properties of the first catalyst are as follows:
[0102] Example 2 uses the same γ-alumina carrier as Example 1. After the carrier is prepared, 4 wt% P2O5 is introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier is 0.96 mL / g and the specific surface area is 269 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 7.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.6% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0103] MoO3, basic nickel carbonate and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0104] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0105] The atomic concentration of Mo in the catalyst is 12atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.785 nm, and the molar ratio of glycerol to Ni is 5.
[0106] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 149m 2 / g, pore volume 0.31cm 3 / g, the average pore diameter is 8.3nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 12.7% of the total pore volume.
[0107] The preparation process and properties of the second catalyst are as follows:
[0108] A γ-alumina carrier was selected, and after the carrier was prepared, 4 wt% P2O5 was introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.96 mL / g, and the specific surface area was 269 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 7.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.6% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0109] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0110] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0111] The atomic concentration of Mo in the catalyst is 3.2atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.3, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.283nm, and the molar ratio of glycerol to Ni is 4.
[0112] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 205m 2 / g, pore volume 0.48cm 3 / g, the average pore size is 9.4nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0113] Performance test of catalyst grading system:
[0114] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 2:1. The reaction temperature of the first catalyst was 359°C and the reaction temperature of the second catalyst was 384°C. After the reaction test, the sulfur content in the product was 3.2ppm and the nitrogen content was 0.8ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.9°C after 5 days of reaction.
[0115] Example 3
[0116] The preparation process and properties of the first catalyst are as follows:
[0117] The same γ-alumina carrier was used in Example 3 as in Example 1. After the carrier was prepared, 6 wt% SiO2 was introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.95 mL / g and the specific surface area was 275 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0118] MoO3, basic nickel carbonate and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a butterfly-shaped catalyst with a particle size of 1.6 mm.
[0119] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0120] The atomic concentration of Mo in the catalyst is 8.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.66 nm, and the molar ratio of glycerol to Ni is 3.
[0121] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 159m 2 / g, pore volume 0.33cm 3 / g, the average pore diameter is 8.3nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 11.5% of the total pore volume.
[0122] The preparation process and properties of the second catalyst are as follows:
[0123] A γ-alumina carrier was selected, and after the carrier was prepared, 6 wt% SiO2 was introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.95 mL / g, and the specific surface area was 275 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0124] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.
[0125] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0126] The atomic concentration of Mo in the catalyst is 3.6atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbonyl group is 0.298 nm, and the molar ratio of glycerol to Ni is 3.
[0127] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 198m 2 / g, pore volume 0.45cm 3 / g, the average pore size is 9.1nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0128] Performance test of catalyst grading system:
[0129] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 1:2. The reaction temperature of the first catalyst was 351°C and the reaction temperature of the second catalyst was 376°C. After the reaction test, the sulfur content in the product was 6.5ppm and the nitrogen content was 1.6ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.1°C after 5 days of reaction.
[0130] Example 4
[0131] The preparation process and properties of the first catalyst are as follows:
[0132] The same γ-alumina carrier was used in Example 4 as in Example 1. After the carrier was prepared, 2 wt% P2O5 was introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.97 mL / g and the specific surface area was 265 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 6.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0133] Ammonium metatungstate, basic nickel carbonate and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 5 hours, and dried at 130°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0134] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0135] The atomic concentration of W in the catalyst is 5.2atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.424 nm, and the molar ratio of citric acid to Ni is 2.
[0136] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 156m 2 / g, pore volume 0.37cm 3 / g, the average pore diameter is 9.5nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 8.5% of the total pore volume.
[0137] The preparation process and properties of the second catalyst are as follows:
[0138] A γ-alumina carrier was selected, and after the carrier was prepared, 2 wt% P2O5 was introduced by impregnation method to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.97 mL / g, and the specific surface area was 265 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 6.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0139] A certain amount of ammonium metatungstate, basic nickel carbonate and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 130°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0140] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0141] The atomic concentration of W in the catalyst is 4atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.35, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.385 nm, and the molar ratio of citric acid to Ni is 2.
[0142] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 168m 2 / g, pore volume 0.39cm 3 / g, the average pore size is 9.3nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0143] Performance test of catalyst grading system:
[0144] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 1:3. The reaction temperature of the first catalyst was 349°C and the reaction temperature of the second catalyst was 374°C. After the reaction test, the sulfur content in the product was 5.3ppm and the nitrogen content was 1.5ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.7°C after 5 days of reaction.
[0145] Example 5
[0146] The preparation process and properties of the first catalyst are as follows:
[0147] A γ-alumina carrier was selected, and 8 wt% SiO2 was introduced during the carrier preparation process to prepare a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.92 mL / g, and the specific surface area was 258 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0148] MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0149] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0150] The atomic concentration of Mo in the catalyst is 9.3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.12, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.64 nm, and the molar ratio of citric acid to Ni is 2.
[0151] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 152m 2 / g, pore volume 0.36cm 3 / g, the average pore diameter is 9.5nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 10.2% of the total pore volume.
[0152] The preparation process and properties of the second catalyst are as follows:
[0153] A γ-alumina carrier was selected and 8 wt% SiO2 was introduced during the carrier preparation process to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.92 mL / g and the specific surface area was 258 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0154] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0155] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0156] The atomic concentration of Mo in the catalyst is 3.8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.32, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.34 nm, and the molar ratio of citric acid to Ni is 2.
[0157] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst was 183m 2 / g, pore volume 0.47cm 3 / g, the average pore size is 10.3nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0158] Performance test of catalyst grading system:
[0159] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 3:1. The reaction temperature of the first catalyst was 361°C and the reaction temperature of the second catalyst was 386°C. After the reaction test, the sulfur content in the product was 3.9ppm and the nitrogen content was 0.9ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.8°C after 5 days of reaction.
[0160] Example 6
[0161] The preparation process and properties of the first catalyst are as follows:
[0162] A γ-alumina carrier was selected, and 1.5 wt% B2O3 was introduced during the carrier preparation process to prepare a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.96 mL / g, and the specific surface area was 274 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0163] MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 2 hours, and dried at 160°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0164] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0165] The atomic concentration of Mo in the catalyst is 9.8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.27, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.83 nm, and the molar ratio of citric acid to Ni is 2.
[0166] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 133m 2 / g, pore volume 0.26cm 3 / g, the average pore diameter is 7.8nm, the pore structure presents a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore diameter of 2-6nm accounts for 10.8% of the total pore volume.
[0167] The preparation process and properties of the second catalyst are as follows:
[0168] A γ-alumina carrier was selected and 1.5 wt% B2O3 was introduced during the carrier preparation process to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.96 mL / g and the specific surface area was 274 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0169] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 160°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0170] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0171] The atomic concentration of Mo in the catalyst is 4.0atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.32 nm, and the molar ratio of citric acid to Ni is 2.
[0172] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 188m 2 / g, pore volume 0.47cm 3 / g, the average pore size is 10.0nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0173] Performance test of catalyst grading system:
[0174] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 1:4. The reaction temperature of the first catalyst was 348°C and the reaction temperature of the second catalyst was 373°C. After the reaction test, the sulfur content in the product was 6.4ppm and the nitrogen content was 1.5ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 1.6°C after 5 days of reaction.
[0175] Comparative Example 1
[0176] The preparation process and properties of the first catalyst are as follows:
[0177] The same modified alumina carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0178] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0179] The atomic concentration of Mo in the catalyst is 3.8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.28, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.322nm, and the molar ratio of glycerol to Ni is 2.
[0180] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 210m 2 / g, pore volume 0.46cm 3 / g, the average pore size is 8.8nm, the pore size distribution of the catalyst is a single-peak pore, and the position of the single-peak pore is 11.4nm.
[0181] The preparation process and properties of the second catalyst are as follows:
[0182] The same modified alumina carrier as in Example 1 was selected to prepare a catalyst. A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0183] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0184] The atomic concentration of Mo in the catalyst is 1.9atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.19, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.161 nm, and the molar ratio of glycerol to Ni is 2.
[0185] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 233m 2 / g, pore volume 0.6cm 3 / g, the average pore size is 10.3nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0186] Performance test of catalyst grading system:
[0187] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 1:1. The reaction temperature of the first catalyst was 355°C and the reaction temperature of the second catalyst was 380°C. After the reaction test, the sulfur content in the product was 26.5ppm and the nitrogen content was 4.6ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.6°C after 5 days of reaction.
[0188] Comparative Example 2
[0189] The preparation process and properties of the first catalyst are as follows:
[0190] The same modified alumina carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0191] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0192] The atomic concentration of Mo in the catalyst is 6.0atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.13, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.38 nm, and the molar ratio of glycerol to Ni is 2.
[0193] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 186m 2 / g, pore volume 0.46cm 3 / g, the average pore diameter is 9.9nm, and the pore structure presents a single-peak pore distribution characteristic, with the single-peak pore appearing at 12.1nm.
[0194] The preparation process and properties of the second catalyst are as follows:
[0195] The same modified alumina carrier as in Example 1 was selected to prepare a catalyst. A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0196] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0197] The atomic concentration of Mo in the catalyst is 2.3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.21, P2O5 / MoO3 molar ratio is 0.22, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.178nm, and the atomic ratio of propylene glycol to Ni is 2.
[0198] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 225m 2 / g, pore volume 0.54cm 3 / g, the average pore size is 9.6nm, and the pore size of the catalyst is in the range of 8-20nm with a single peak pore distribution.
[0199] Performance test of catalyst grading system:
[0200] The first catalyst and the second catalyst were compounded and loaded in a volume ratio of 2:1. The reaction temperature of the first catalyst was 359°C and the reaction temperature of the second catalyst was 384°C. After the reaction test, the sulfur content in the product was 19.3ppm and the nitrogen content was 3.5ppm. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 3.2°C after 5 days of reaction.
[0201] It can be seen from the examples and comparative examples that the catalyst grading system provided by the present invention has higher hydrodesulfurization and denitrification performance and has good industrial application prospects.
[0202] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydrodesulfurization and denitrification catalyst grading system, the grading system comprising a first catalyst and a second catalyst arranged in sequence along a logistics direction; The first catalyst comprises a metal element of Group VIII, a metal element of Group VIB and a modified alumina carrier, and has a pore volume of 0.15-0.5 cm 3 / g, average pore size is 6-15nm, in, The pore size of the catalyst presents a bimodal pore distribution in the range of 2-6 nm and 8-20 nm; The second catalyst comprises a modified alumina carrier and a metal element of Group VIII, a metal element of Group VIB and a phosphorus element supported on the modified alumina carrier, and has a pore volume of 0.3-0.55 cm 3 / g, with an average pore size of 7-15nm, wherein the pore size of the second catalyst presents a unimodal pore distribution in the range of 8-20nm; The modified alumina supports in the first catalyst and the second catalyst each independently contain a weakly acidic component; The weakly acidic component is selected from at least one of B, P, Si, F and Ge elements; In the modified alumina carrier, the content of the weakly acidic component is 0.5-10% by weight, calculated as oxide; In the first catalyst, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for 7-15% of the total pore volume of the catalyst.
2. The grading system according to claim 1, in, In the modified alumina carrier, B 2 O 3 The content is not more than 5% by weight, or P 2 O 5 The content is not more than 6% by weight, or SiO 2 The content is not more than 10% by weight, or the F content is not more than 5% by weight, or GeO 2 The content is not more than 6% by weight.
3. The grading system according to claim 1 or 2, in, The water absorption rate of the alumina in the modified alumina carrier is greater than 0.9 mL / g, and the specific surface area is greater than 250 m 2 / g, the average pore size is greater than 9nm, and the pore distribution morphology is a unimodal pore distribution.
4. The grading system according to claim 1 or 2, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the modified alumina carrier.
5. The grading system according to claim 4, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 8% of the total pore volume of the modified alumina carrier.
6. The grading system according to claim 1 or 2, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 4% of the total pore volume of the modified alumina carrier.
7. The grading system according to claim 1 or 2, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 3% of the total pore volume of the modified alumina carrier.
8. The grading system according to claim 1 or 2, in, In the first catalyst, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for 8-13% of the total pore volume of the catalyst.
9. The grading system according to claim 1 or 2, in, The first catalyst composition is (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the modified alumina support Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the modified alumina support Yi, and Zi is P 2 O 5 , ci is relative to 1 gram of modified alumina support P 2 O 5 The mass of Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-1nm, ρ Xi , Yi , Zi are Group VIB metal oxides, Group VIII metal oxides and P 2 O 5 The density of SA sup is the specific surface area of the modified alumina carrier.
10. The grading system according to claim 9, in, The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.4-0.85nm.
11. The grading system according to claim 10, in, The molar ratio of Zi / Xi in the first catalyst is 0.1-0.
4.
12. The grading system according to claim 11, in, The molar ratio of Zi / Xi in the first catalyst is 0.1-0.
35.
13. The grading system according to claim 1 or 2, in, The second catalyst composition is (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the modified alumina support Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the modified alumina support Yi, and Zi is P 2 O 5 , ci is relative to 1 gram of modified alumina support P 2 O 5 The mass of Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.2-0.39nm, ρ Xi , Yi , Zi are Group VIB metal oxides, Group VIII metal oxides and P 2 O 5 The density of SA sup is the specific surface area of the modified alumina carrier.
14. The grading system according to claim 13, in, The molar ratio of Zi / Xi in the second catalyst is 0.05-0.45:
1.
15. The grading system according to claim 14, in, The molar ratio of Zi / Xi in the second catalyst is 0.2-0.38:
1.
16. The grading system according to claim 1 or 2, in, The atomic concentration of the VIB group metal element in the first catalyst on the surface of the modified alumina carrier is 4.5-14 atom / nm 2 ; and / or, the atomic concentration of the metal element of Group VIB in the second catalyst on the surface of the modified alumina carrier is 2-5.5atom / nm 2 .
17. The grading system according to claim 16, in, The atomic concentration of the VIB group metal element in the first catalyst on the surface of the modified alumina carrier is 5-12 atom / nm 2 .
18. The grading system according to claim 16, in, The atomic concentration of the VIB group metal element in the second catalyst on the surface of the modified alumina carrier is 3-4.5 atom / nm 2 .
19. The grading system according to claim 1 or 2, in, The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the first catalyst is 0.1-0.4; and / or, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the second catalyst is 0.2-0.
38.
20. The grading system according to claim 19, in, The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the first catalyst is 0.2-0.
3.
21. The grading system according to claim 19, in, The atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the second catalyst is 0.2-0.
3.
22. The grading system according to claim 1 or 2, in, The first catalyst and the second catalyst each independently further include an organic alcohol compound and / or a carboxylic acid compound.
23. The grading system according to claim 22, in, In the first catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is 1-6.
24. The grading system according to claim 23, in, In the first catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is 2-5.
25. The grading system according to claim 22, in, In the second catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is 1-4.
26. The grading system according to claim 25, in, In the second catalyst, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is 2-4.
27. The grading system according to claim 1 or 2, in, The packing volume ratio of the first catalyst to the second catalyst is 1:4-4:
1.
28. The grading system according to claim 27, in, The packing volume ratio of the first catalyst to the second catalyst is 1:3-3:
1.
29. The grading system according to claim 1 or 2, in, The equivalent diameters of the first catalyst and the second catalyst are each independently 0.5-1.8 mm.
30. The grading system according to claim 29, in, The equivalent diameters of the first catalyst and the second catalyst are each independently 0.8-1.6 mm.
31. The grading system according to claim 1 or 2, in, The shapes of the first catalyst and the second catalyst are independently cylindrical, three-leaf clover, four-leaf clover, honeycomb or other irregular shapes.
32. The grading system according to claim 1 or 2, in, The preparation methods of the first catalyst and the second catalyst independently include: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound and optionally an organic alcohol compound and / or a carboxylic acid compound into a modified alumina carrier by an impregnation method, and then drying.
33. A method for hydrodesulfurization and denitrification, the method include: The distillate oil to be treated is reacted with the grading system according to any one of claims 1 to 32 under hydrodesulfurization and denitrogenation conditions.
34. The method for hydrodesulfurization and denitrification according to claim 33, in, The distillate oil to be treated has a sulfur content of 4000-15000 ppm and a nitrogen content of 200-3000 ppm.
35. The method for hydrodesulfurization and denitrification according to claim 33 or 34, in, The hydrodesulfurization and denitrification conditions include: temperature of 300-420°C, pressure of 5-15 MPa, volume space velocity of 0.5-10 hours -1 , the volume ratio of hydrogen to oil is 250-2000:1.