A method for resurrecting spent catalytic cracking catalyst

By easing the devanadium and aluminum coating treatments, the problems of poor activity stability and anti-pollution performance in the regeneration of spent catalytic cracking catalysts are solved, and efficient catalyst regeneration and heavy oil conversion effects are achieved.

CN116060141BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111267520.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-11
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

It is difficult to effectively resurrect spent catalytic cracking catalysts with existing technology, especially catalysts with high pollution metal content, resulting in poor activity stability and low crystallinity after resurrection, and it is difficult to obtain highly active catalysts after deep demetallization.

Method used

By easing the devanadium treatment and aluminum coating activity protection, the vanadium content is controlled within an appropriate range, and combined with the aluminum compound dispersion and ammonium fluorosilicate treatment, an aluminum compound coating is formed to improve the activity stability and anti-pollution performance of the catalyst.

Benefits of technology

It significantly improves the activity stability and crystallinity of the resurrection catalyst, enhances the anti-pollution performance, reduces the ratio of hydrogen to methane, and improves the heavy oil conversion capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003327296980000081
    Figure BDA0003327296980000081
  • Figure BDA0003327296980000082
    Figure BDA0003327296980000082
  • Figure BDA0003327296980000091
    Figure BDA0003327296980000091
Patent Text Reader

Abstract

The present invention belongs to the field of environmental protection technology and relates to a method for resurrecting a catalytic cracking waste catalyst, comprising: (S1) treating the catalytic cracking waste catalyst to obtain a first waste catalyst; (S2) contacting the first waste catalyst with an aluminum compound dispersion; wherein Al 2 O 3 The weight ratio of the aluminum compound dispersion to the catalytic cracking spent catalyst on a dry basis is 0.1 to 5:100; the aluminum compound dispersion is Al 2 O 3 The aluminum compound content is preferably 0.03 to 15% by weight; (S3) calcining. This method can passivate the polluted metal, improve the strength of the catalyst, and increase the activity stability of the revived catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental protection and relates to a method for reviving a catalytic cracking waste catalyst with passivated polluted metals. Background Art

[0002] Since the operation of the first industrial fluid catalytic cracking unit in 1942, catalytic cracking has developed into the core processing technology in refineries, the most important secondary processing process, and an important means to improve the depth of crude oil processing and increase the yield of light oil. As crude oil becomes heavier and inferior, FCC catalysts are more susceptible to coking, poisoning and hydrothermal deactivation. In order to meet the needs of the unit and maintain the catalytic cracking performance of the catalyst, it is necessary to regularly unload part of the waste catalyst (i.e., FCC balance) and replenish fresh catalyst. Therefore, major domestic refineries produce a large amount of FCC waste catalyst every year. Underground burial is a relatively easy way to treat waste catalysts, but it not only wastes resources but also pollutes the environment. Therefore, it is urgent to study the resurrection and reuse of FCC waste catalysts.

[0003] At present, the main methods for resurrecting FCC spent catalysts are: magnetic separation and chemical regeneration.

[0004] Magnetic separation is the use of magnetic separation technology to revive waste catalysts contaminated by heavy metals. FCC balance agent particles that have been deactivated by metal poisoning show a certain degree of magnetism under a magnetic field. The magnetic separation method can be used to separate particles with a large amount of heavy metals deposited in the balance agent, thereby reducing the heavy metal content of the balance agent, improving its reaction performance, and meeting the requirements of the device for the reuse of the balance agent. However, it can only be used to treat balance agents with a relatively low degree of heavy metal contamination (Petroleum Refining and Chemical Industry, 2003, 34(8), 20).

[0005] Chemical regeneration is to remove heavy metals deposited on the waste catalyst by chemical methods, thereby improving the cracking activity of the balancer. Among them, the acid washing method is currently the most commonly used resurrection technology. It includes the removal of heavy metals in the balancer by inorganic acids such as hydrochloric acid, sulfuric acid, and nitric acid (Journal of Petroleum University, 2005, 29 (4), 115), the removal of heavy metals by organic acids through coordination reactions (Petroleum Refining and Chemical Industry, 2006, 37 (11), 11) and the resurrection of FCC waste catalysts by inorganic-organic coupling methods. CN101219396A discloses a method for the coordinated resurrection of FCC waste catalysts by inorganic acids and organic acids, and the micro-reaction activity of the catalyst after resurrection can be increased by more than 10 points. The stability of the resurrected catalyst obtained by the above method is poor, and the activity after aging is not high. The above method does not improve the crystallinity and activity stability of the catalyst.

[0006] In the prior art, catalytic cracking waste catalysts usually contain contaminated metals. If the content of contaminated metals is high, the dehydrogenation activity of the revived catalyst is high. If deep demetallization is performed, it is not easy to obtain a highly active revived catalyst. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for resurrecting spent catalytic cracking catalysts. The resurrected catalysts obtained by the method are resistant to metal pollution and have a low hydrogen / methane ratio.

[0008] The inventors of the present invention have found that the activity of catalytic cracking waste catalysts containing V often decreases and is usually not suitable for reuse. The vanadium content of the catalyst can be reduced by devanadiumization, but often when the vanadium content is not very low, the adverse effects of vanadium cannot be completely eliminated. When the vanadium content is reduced a lot in the conventional way, the structure of the catalyst is often destroyed, and the activity stability of the revived catalyst is not high. For this reason, the inventors have creatively proposed a method for moderate vanadium reduction and resurrection. The method treats a catalyst with a vanadium content within a suitable range or a high vanadium content by moderate devanadiumization to make the vanadium content within a suitable range, and then performs an aluminum coating activity protection treatment, which can effectively control the destructive effect of residual vanadium and stabilize the activity of the catalyst.

[0009] The present invention provides a method for resurrecting a catalytic cracking waste catalyst containing polluted metals, comprising:

[0010] (S1) treating a catalytic cracking waste catalyst to obtain a first waste catalyst; the first waste catalyst may have a V content of 0.3 to 0.6 wt %;

[0011] (s2) contacting the first spent catalyst with a dispersion of an aluminum compound to obtain a first contact mixture;

[0012] The weight ratio of the aluminum compound dispersion calculated as Al2O3 to the catalytic cracking waste catalyst on a dry basis is 0.1 to 5:100; the aluminum compound content calculated as Al2O3 in the aluminum compound dispersion is preferably 0.03 to 15% by weight;

[0013] (S3) The first contact mixture is calcined, or dried and then calcined.

[0014] According to the method for resurrecting a spent catalytic cracking catalyst of the present invention, the aluminum compound dispersion can be an aluminum compound solution and / or aluminum gel. The method for contacting the first spent catalyst with the aluminum compound dispersion is as follows: contacting the first spent catalyst with the aluminum compound solution and / or aluminum gel; the contact is carried out by dipping, leaching, spraying or deposition; preferably, the aluminum oxide (calculated as Al2O3) introduced by the contact accounts for 0.1-5 weight % or 1-5 weight % or 0.1-2 weight % of the dry weight of the resurrected catalyst obtained.

[0015] According to the method for resurrecting spent catalytic cracking catalyst of the present invention, the aluminum compound solution includes but is not limited to an aqueous solution of one or more of aluminum chloride, aluminum sulfate, organic aluminum, aluminum nitrate, and macromolecular complex aluminum salts; the aluminum colloid is preferably aluminum sol and / or acidified pseudo-boehmite.

[0016] According to the method of the present invention, wherein, optionally, the aluminum compound dispersion contains an additive, the additive is a macromolecular surfactant and / or an organic macromolecular micelle. The additive is, for example, one or more of a linear polymer, cellulose, lignin, sodium carboxymethyl cellulose, starch, short polyethylene, short polypropylene, and polyacrylamide. Preferably, the additive accounts for 0.01 wt % to 10 wt % of the aluminum compound dispersion (calculated as the aluminum oxide therein).

[0017] In one embodiment, the aluminum compound is introduced by deposition. The aluminum compound dispersion is an aluminum salt solution, and the first waste catalyst can be mixed with the aluminum compound dispersion, and then ammonia water is added to adjust the pH value of the dispersion to 9-11, and optionally filtered to obtain a first contact mixture.

[0018] According to the method for resurrecting a catalytic cracking waste catalyst of the present invention, the first waste catalyst is contacted with an aluminum compound dispersion, and the temperature of the first waste catalyst is 0 to 200° C., for example, 90 to 200° C.; in the step (S2), the calcination temperature is preferably 400 to 550° C., and the calcination time is preferably 1 to 3 hours.

[0019] According to the method for resurrecting a spent catalytic cracking catalyst of the present invention, the treatment in step (S1) includes a first resurrection treatment, and the first resurrection treatment may be one or more of weak acid washing, ammonium exchange, phosphorus treatment or a second resurrection treatment. When multiple treatment methods are included, the order of the multiple resurrection treatments is not limited. The treatment optionally includes the step of a mild demetallization treatment. In one embodiment, the mild devanadiumization method is as follows: using a weak acid or a weak base, such as ammonium treatment, to remove part of the metal without destroying the crystal structure of the active component. Preferably, the first resurrection treatment includes a second resurrection treatment, and optionally includes a third resurrection treatment, such as one or more of weak acid washing, ammonium exchange, and phosphorus treatment.

[0020] The second resurrection process comprises the following processing steps:

[0021] (1) contacting (NH4)2SiF6, an optional buffer, and a calcined catalytic cracking waste catalyst in water for reaction, and heat treating the mixture at a temperature of 70 to 150° C. for more than 1 hour to obtain a first slurry;

[0022] (2) The first slurry obtained in step (1) is filtered and washed to obtain the washed catalytic cracking waste catalyst. Some heavy metals in the catalytic cracking waste catalyst can be removed, the reconstruction of the catalyst structure is promoted, the crystallinity is improved, and the activity stability of the revived catalyst is improved. The activity of the revived catalyst decreases less after aging.

[0023] According to the method for resurrecting a spent catalytic cracking catalyst of the present invention, the liquid-to-solid ratio of the mixture formed by the (NH4)2SiF6, buffer, calcined spent catalytic cracking catalyst and water can be 10-40:1, for example, 20-40:1; the liquid-to-solid ratio is the ratio of the total weight of the (NH4)2SiF6, buffer and water to the weight of the spent catalytic cracking catalyst after calcination on a dry basis, and the weight of the spent catalytic cracking catalyst after calcination is on a dry basis.

[0024] In step (1), the weight ratio of the buffer to the calcined catalytic cracking waste catalyst is preferably 3 to 7:1, and the weight of the calcined catalytic cracking waste catalyst is calculated on a dry basis.

[0025] The weight ratio of the molar number of ammonium fluorosilicate to the calcined spent catalytic cracking catalyst is preferably 0.0004-0.008 mol / g, such as 0.0005-0.005 mol / g, the weight of the calcined spent catalytic cracking catalyst being on a dry basis.

[0026] According to the method for resurrecting a spent catalytic cracking catalyst of the present invention, a preferred embodiment is to form a slurry (called a second slurry) with the calcined spent catalytic cracking catalyst, a buffer and water, add a (NH4)2SiF6 solution to the second slurry at a temperature of 70 to 90°C, and then perform a heat treatment. The resurrected catalyst obtained in this way has a better heavy oil conversion effect.

[0027] Preferably, the weight ratio of the total weight of the buffer and water in the second slurry to the calcined catalytic cracking waste catalyst (on a dry basis) is 15 to 35:1; the dripping time of the NH4)2SiF6 solution is 60 to 180 min, preferably 75 to 150 min, the heat treatment temperature is 70 to 150°C, for example, 70-90°C or 100 to 150°C, the heat treatment time is 1 to 24h or 5 to 24 hours or 2 to 5 hours, for example, heat treatment at 100 to 150°C for 2 to 5 hours or heat treatment at a temperature of 70-90°C for 5 to 24 hours.

[0028] In one embodiment, the heat treatment is performed by stirring at 70 to 150° C. for 1 to 24 hours.

[0029] In one embodiment, the amount of the ammonium fluorosilicate solution added is 3-7 mL / g of the calcined catalytic cracking waste catalyst (on a dry basis), and the concentration of the ammonium fluorosilicate solution is preferably 0.1-1.0 mol / L, preferably 0.2-0.6 mol / L.

[0030] According to the method for resurrecting a spent catalytic cracking catalyst of the present invention, in one embodiment, in the second slurry, the weight ratio of the total weight of the buffer and water to the spent catalytic cracking catalyst after calcination (on a dry basis) is 15 to 35:1, and the weight ratio of the total weight of the buffer and water to the spent catalytic cracking catalyst after calcination on a dry basis is preferably 20 to 30:1. The percentage of the buffer to the total weight of the buffer and water is 15 to 25 weight %, such as 18 weight %, 20 weight % or 22 weight %.

[0031] The calcined catalyst cracking waste catalyst in step (1) refers to the catalyst cracking waste catalyst being calcined, and the calcination can be carried out at a temperature of 500-800° C., preferably 600-800° C., for 1-3 hours in an air atmosphere. The calcination can oxidize the vanadium on the catalyst into a high-valent state, thereby increasing the probability of vanadium removal.

[0032] The catalytic cracking waste catalyst is an existing catalytic cracking waste catalyst. In one embodiment, the catalytic cracking waste catalyst contains a molecular sieve such as a Y-type molecular sieve, and the vanadium content is 0.4-0.8% by weight as V2O5, and the nickel content is 0-0.8% by weight as NiO. The catalytic cracking waste catalyst is usually a waste catalyst or a balance discharged from a catalytic cracking unit, and is preferably calcined to obtain a calcined catalytic cracking waste catalyst for the treatment in step (1).

[0033] According to the method for resurrecting spent catalytic cracking catalyst of the present invention, the buffer is a substance that can form a buffer solution with a pH value of 5 to 8, preferably 6 to 7, with water, and can be selected from organic acid ammonium, such as ammonium salts of organic acids with a carbon number less than 4 in the molecule, preferably one or more of ammonium oxalate, ammonium formate, ammonium acetate, etc., more preferably ammonium acetate.

[0034] The washing in step (2) is to remove the removed vanadium ions and excess ammonium ions. The washing method is well known to those skilled in the art, for example, washing with deionized water at 80-100°C, washing once or multiple times, for example, washing 1-3 times, and the weight ratio of deionized water to filter cake base in each washing can be 5-15:1.

[0035] The product of step (2) can be used directly as the first waste catalyst, or further comprises step (3): subjecting the product of step (2) to a third treatment, such as one or more of an acid solution, phosphorus modification, and ammonia washing resurrection treatment.

[0036] According to the method for resurrecting a spent catalytic cracking catalyst of the present invention, an aluminum compound coating is formed on the surface of the resurrected catalyst by contacting and calcining in (S2); the aluminum compound coating accounts for 0.1 to 5% by weight of the dry weight of the obtained resurrected catalyst in terms of alumina. The coating thickness is preferably D / 3000 to D / 30 of the diameter of the resurrected catalyst particles, where D is the diameter of each particle. In one embodiment, the diameter D of the resurrected catalyst is 20 to 140 μm, and the average diameter is 60 to 80 μm. The coating thickness and particle diameter can be detected by scanning electron microscopy of the cross section of the catalyst microspheres.

[0037] In the step (S3), the calcination temperature is preferably 400-550° C. and the calcination time is preferably 1-3 hours.

[0038] The phosphorus modification is, for example, placing the catalytic cracking waste catalyst or the revived catalytic cracking waste catalyst in a solution containing a phosphorus compound, wherein the phosphorus compound can be selected from one or more of phosphoric acid, pyrophosphoric acid, phosphorous acid, ammonium phosphate, and alkali metal phosphate.

[0039] The ammonium exchange is, for example, that the catalytic cracking waste catalyst or the revived catalytic cracking waste catalyst is placed in a solution containing ammonia or an ammonium salt, and stirred at 40 to 90° C. for 0.1 to 3 hours. The ammonium salt is, for example, one or more of ammonium sulfate, ammonium chloride, ammonium phosphate and ammonium hydrogen phosphate, but is not limited thereto. The ammonium exchange can be performed once or multiple times, for example, once to twice.

[0040] The acid washing process is as follows: the catalytic cracking waste catalyst or the revived catalytic cracking waste catalyst that has been revived and modified is placed in an acid solution with a pH of 3 to 5, at 60 to 90° C., and stirred for 0.1 to 3 hours. The acid used can be selected from one or more of hydrochloric acid, nitric acid, phosphoric acid, sulfuric acid, oxalic acid, and citric acid. The acid washing process can be performed once or multiple times, for example, once to twice.

[0041] The present invention provides a resurrection catalyst, which is prepared by the method described in any one of the technical solutions of the present invention.

[0042] The method for resurrecting a spent catalytic cracking catalyst of the present invention is simple in method and mild in reaction conditions, and can improve the activity stability of the resurrected catalyst, for example, the activity of the resurrected catalyst decreases less after aging, improve the strength of the resurrected catalyst, and enhance the anti-pollution metal performance of the resurrected catalyst, for example, the ratio of hydrogen to methane in light oil conversion can be reduced.

[0043] The resurrection catalyst provided by the present invention can have a higher crystallinity, good activity stability, and strong heavy oil cracking ability. Preferably, compared with the resurrection catalyst obtained by the existing resurrection method, the resurrection catalyst obtained by the method of the present invention can have a higher crystallinity, improved strength, and can have good resistance to metal pollution and higher heavy oil conversion activity under the condition of higher activity stability. It can be used for heavy oil conversion and can have a lower hydrogen rate or hydrogen-methane ratio. For example, the catalytic cracking waste catalyst resurrection method provided by the present invention can have a vanadium removal rate of more than 20%, and the activity after aging at 780°C and 100% water vapor / 8h can be increased by more than 10 percentage points relative to the blank agent. The obtained resurrection catalyst has enhanced metal resistance, can passivate the resurrection catalyst and neutralize newly deposited nickel and vanadium, and can be used for heavy oil conversion, with a lower hydrogen-methane ratio. DETAILED DESCRIPTION

[0044] In one embodiment, the present invention provides a method for resurrecting a waste catalytic cracking catalyst containing polluted metals, comprising the following steps:

[0045] (1) contacting and reacting (NH4)2SiF6, a buffer, and a calcined catalytic cracking waste catalyst in water, and then heat-treating the mixture at a temperature of 70 to 150° C. to obtain a first slurry;

[0046] (2) filtering the first slurry obtained in step (1), and washing to remove the removed metal ions (such as vanadium) and most of the ammonium ions, to obtain a washed catalytic cracking spent catalyst;

[0047] (3) subjecting the washed catalytic cracking waste catalyst to an aluminum sol coating treatment, that is, aluminum forms an aluminum sol coating on the surface of the treated waste catalyst;

[0048] (4) filtering the slurry obtained in step (3), drying and calcining to obtain a revived catalyst.

[0049] The following examples will further illustrate the present invention and are intended to help readers better understand the essence of the present invention and the beneficial effects brought about, but should not be construed as any limitation on the practicable scope of the present invention.

[0050] The crystal structure of the sample was characterized by X'Pert X-ray powder diffractometer from PHILIPS Company, Cu Kα radiation, tube voltage 40kV, tube current 40mA, scanning speed 2(°) / min, scanning range 5°~70°.

[0051] The ASAP 2405N V1.01 automatic adsorption instrument from Micromeritics of the United States was used, and the low-temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10 -2The sample was vacuum degassed at 300°C for 4 h, and N2 was used as the adsorption medium to measure the adsorption-desorption isotherm of the sample at 77.4 K. The specific surface area (SBET) of the sample was calculated according to the BET formula, and the volume of N2 adsorbed by the sample at the relative pressure p / p0=0.98 was measured and converted into liquid nitrogen volume, i.e., the total pore volume.

[0052] Micro-reaction activity index: The standard method of RIPP92-90 (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990) was used to evaluate the light oil micro-reaction activity of the sample. The catalyst loading was 5.0 g, the reaction temperature was 460°C, the feed oil was straight-run light diesel with a distillation range of 235-337°C, and the product composition was analyzed by gas chromatography. The light oil micro-reaction activity was calculated based on the product composition.

[0053] Strength: that is, the wear index of catalytic cracking catalyst, measured according to the NB / SH / T 0964-2017 method.

[0054] The FCC waste catalyst (denoted as CAT0) has a composition as shown in Table 1, contains Y-type molecular sieve, and is sourced from the third catalyst of Yanshan Petrochemical. The FCC waste catalyst was calcined at a temperature of 700° C. in an air atmosphere for 2 h to obtain a calcined FCC waste catalyst.

[0055] Example 1

[0056] (1) 30 g of calcined FCC waste catalyst (on a dry basis) was added to 600 g of deionized water and 150 g of solid ammonium acetate. The mixture was stirred at 90° C. and 150 mL of a 0.5 mol / L ammonium fluorosilicate solution was slowly added dropwise for 100 min. After the addition was completed, the mixture was stirred at 90° C. for 20 min. The mixture was heated to 120° C. and heat treated for 3 h (in an autoclave). The mixture was filtered, washed with 300 mL of boiling water, and dried to obtain catalyst CAT1. (2) A sol suspension of 15 g of an acidified pseudo-boehmite sol (acid-aluminum ratio (HCl:Al2O3 molar ratio) of 12:100) with a concentration of 6 wt% based on alumina and 0.2 wt% (based on alumina) of sodium carboxymethyl cellulose was sprayed onto the catalyst CAT1 at 150°C, stirred thoroughly while spraying, and then dried at 120°C for 0.5 h and calcined at 500°C for 2 h to obtain a resurrected catalyst with 3% alumina loaded on the outer surface of CAT1. Through cross-sectional electron microscopy analysis, it was clearly seen that there was an alumina coating on the surface with an average thickness of 0.8 μm, denoted as FCAT1. The physicochemical properties are detailed in Table 1. Thickness measurement: Three particles were randomly selected, and three radial lines were randomly selected from the cross section of each particle to measure the thickness. The average value was taken as the average thickness.

[0057] Example 2

[0058] (1) Take 30 g of the calcined FCC waste catalyst (on a dry basis), add 600 g of deionized water, add 150 g of solid ammonium acetate, stir at 90° C., and slowly drop 150 mL of a 0.5 mol / L ammonium fluorosilicate solution for 100 min. After the dropwise addition is completed, continue stirring at 90° C. for 20 min, heat to 120° C. for 3 h, filter, wash with 300 mL of boiling water, and dry to obtain CAT2. (2) After 100 g of aluminum chloride solution (1 wt% in terms of alumina) and 30 g of CAT2 were fully stirred at 30° C. for 30 min, ammonia water was added to adjust the pH to 10, stirring was continued and filtering was performed. The solid matter on the filter cloth was fully stirred and dried, and calcined at 500° C. for 2 h to obtain a resurrected catalyst in which CAT2 was loaded with about 0.15% alumina. By cross-sectional electron microscopy analysis, it was found that there was an alumina-enriched layer on the surface with an average thickness of 0.6 μm, which was denoted as FCAT2. The physicochemical properties are shown in Table 1.

[0059] Example 3

[0060] The method of reference example 1 was used, except that ammonium acetate was not added, to obtain a revived catalyst, which was recorded as FCAT3.

[0061] Example 4

[0062] The method of Example 1 was used with reference to that of Example 1, except that the ammonium fluorosilicate was added quickly within 1 minute to obtain a revived catalyst, which was recorded as FCAT4.

[0063] Example 5

[0064] 30 g of FCC waste catalyst was added to a three-necked flask, and 240 g of hydrochloric acid solution with a pH value of 1 was added under stirring, and the mixture was heated to 80°C. Then, 150 g of 0.05 mol of oxalic acid solution was added, and the reaction was maintained at 80°C for 8 hours. After the reaction was completed and the mixture was naturally cooled to room temperature, the product was filtered and washed until the pH value of the filtrate was about 7. The washed product was dried at 100°C for 24 hours to obtain a revived catalyst, which was recorded as dCAT1. (2) 15 g of a liquid mixed with 6% acidified pseudo-boehmite and 0.2% short polypropylene in terms of alumina was sprayed on catalyst CAT5 at 150°C, with sufficient stirring during spraying, and then dried at 120°C for 0.5 h, and calcined at 500°C for 2 h to obtain a revived catalyst with about 3% alumina loaded on the outer surface of CAT5. By cross-sectional electron microscopy analysis, it was clearly seen that there was an alumina coating on the surface with an average thickness of 0.8 μm, which was recorded as FCAT5. The physicochemical properties are shown in Table 1. The physicochemical properties are shown in Table 1.

[0065] Comparative Example 1

[0066] Take 30 grams of calcined FCC waste catalyst (on a dry basis), add 600 grams of deionized water, add 150 grams of solid ammonium acetate, stir at 90°C, and slowly add 150 mL of 0.5 mol / L ammonium fluorosilicate solution for 100 minutes. After the addition is completed, continue stirring at 90°C for 20 minutes, heat to 120°C for 3 hours, filter, wash with 300 mL of boiling water, and dry to obtain a revived catalyst, recorded as DFCAT1. The physicochemical properties are shown in Table 1.

[0067] Table 1

[0068]

[0069] After the catalyst was aged at 780°C and 100% by volume steam for 8 h, its catalytic cracking performance was evaluated in a small fixed fluidized bed reactor (ACE). The properties of the feedstock oil in the ACE experiment are shown in Table 2, and the evaluation results are listed in Table 3.

[0070] Table 2 Raw oil properties

[0071]

[0072]

[0073] Table 3

[0074]

[0075] As can be seen from Table 1, the revived catalyst obtained by the method of the present invention has increased strength and more stable activity after aging.

[0076] As can be seen from Table 3, the catalytic cracking catalyst resurrection method adopted in the present invention increases the strength of the resurrected catalyst, enhances the heavy metal resistance, and shows improved product distribution, such as a decrease in the H2 / CH4 molar ratio. Preferably, the conversion rate is increased and the gasoline yield is increased.

Claims

1. A method for resurrecting a catalytic cracking waste catalyst containing polluted metals, comprising: (S1) treating a catalytic cracking waste catalyst to obtain a first waste catalyst; the catalytic cracking waste catalyst contains a molecular sieve, and the V content of the first waste catalyst is 0.3-0.6 wt % or the V content of the first waste catalyst is 0.4-0.8 wt %; The treatment includes a first resurrection treatment; the first resurrection treatment includes a second resurrection treatment and optionally includes a third resurrection treatment; The second resurrection process comprises the following processing steps: (1) contacting (NH4)2SiF6, a buffer, and a calcined catalytic cracking waste catalyst in water for reaction, and heat treating the mixture at a temperature of 70 to 150° C. for more than 1 hour to obtain a first slurry; (2) filtering and washing the first slurry obtained in step (1) to obtain washed catalytic cracking waste catalyst; The third resurrection treatment is one or more of weak acid washing, ammonium exchange, and phosphorus treatment; (S2) contacting a first spent catalyst with an aluminum compound dispersion to obtain a first contact mixture; The weight ratio of the aluminum compound dispersion calculated as Al2O3 to the catalytic cracking waste catalyst calculated as dry basis is 0.1-5:100; the aluminum compound content calculated as Al2O3 in the aluminum compound dispersion is 0.03-15% by weight; the contacting method of the first waste catalyst with the aluminum compound dispersion is as follows: the first waste catalyst is contacted with the aluminum compound solution and / or aluminum gel, and the contacting is carried out by dipping, leaching, spraying or deposition; (S3) The first contact mixture is calcined or dried and then calcined.

2. The method for resurrecting a spent catalytic cracking catalyst according to claim 1, characterized in that: The alumina introduced by the contact accounts for 1 to 5 weight % of the dry weight of the revived catalyst obtained.

3. The method for resurrecting a spent catalytic cracking catalyst according to claim 2, characterized in that: The aluminum compound solution is an aqueous solution of one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, organic aluminum, and macromolecular complex aluminum salt; the aluminum colloid is aluminum sol and / or acidified pseudo-boehmite.

4. The method according to claim 1, characterized in that: The aluminum compound dispersion contains an additive, which is a macromolecular surfactant and / or an organic macromolecular micelle. The additive accounts for 0.01 wt % to 10 wt % of the aluminum compound dispersion calculated as aluminum oxide.

5. The method for resurrecting spent catalytic cracking catalyst according to claim 1, characterized in that: The first waste catalyst is contacted with the aluminum compound dispersion, and the temperature of the first waste catalyst is 0-200°C; the calcination in step (S3) is performed at a temperature of 400-550°C.

6. The method for resurrecting spent catalytic cracking catalyst according to claim 4, characterized in that: The additive is one or more of linear polymer, cellulose, lignin, sodium carboxymethyl cellulose, starch, short polyethylene, short polypropylene, and polyacrylamide.

7. The method for resurrecting spent catalytic cracking catalyst according to claim 1, characterized in that: In the mixture formed by the (NH4)2SiF6, buffer, calcined catalytic cracking waste catalyst and water, the liquid-to-solid ratio is 10-40:1; the weight ratio of the buffer to the calcined catalytic cracking waste catalyst is 3-7:1, the weight ratio of the molar number of ammonium fluorosilicate to the calcined catalytic cracking waste catalyst is 0.0004-0.008 mol / g, and the weight of the calcined catalytic cracking waste catalyst is calculated on a dry basis; the liquid-to-solid ratio is the weight ratio of the total weight of (NH4)2SiF6, buffer and water to the weight of the calcined catalytic cracking waste catalyst calculated on a dry basis.

8. The method for resurrecting spent catalytic cracking catalyst according to claim 1, characterized in that: The calcined catalytic cracking waste catalyst, a buffer and water are used to form a second slurry, and a (NH4)2SiF6 solution is added to the slurry at a temperature of 70 to 90°C, wherein the weight ratio of the total weight of the buffer and water in the second slurry to the weight of the calcined catalytic cracking waste catalyst on a dry basis is 15 to 35:1; the addition time of the (NH4)2SiF6 solution is 60 to 180 minutes; and then a heat treatment is performed at a temperature of 70 to 150°C and a heat treatment time of 1 to 24 hours.

9. The method for resurrecting spent catalytic cracking catalyst according to claim 8, characterized in that: The addition time of (NH4)2SiF6 solution is 75 to 150 minutes. After the addition of (NH4)2SiF6 solution, stir at 70 to 150°C for 1 to 24 hours.

10. The method for resurrecting spent catalytic cracking catalyst according to claim 8 or 9, characterized in that: The amount of the ammonium fluorosilicate solution added is 3-7 mL / g of the calcined catalytic cracking waste catalyst on a dry basis, and the concentration of the ammonium fluorosilicate solution is 0.1-1.0 mol / L.

11. The method for resurrecting spent catalytic cracking catalyst according to claim 1, 8 or 9, characterized in that: The weight ratio of the total amount of buffer and water to the calcined catalytic cracking waste catalyst is 20-30 g / g of the calcined catalytic cracking waste catalyst, the percentage of buffer to the total weight of buffer and water is 15-25% by weight, and the weight of the calcined catalytic cracking waste catalyst is calculated on a dry basis.

12. The method for resurrecting spent catalytic cracking catalyst according to claim 1 or 7, characterized in that: The buffer is a substance that can form a buffer solution with a pH value of 5 to 8 with water, and is selected from organic acid ammonium.

13. The method according to claim 1, characterized in that The first waste catalyst is the product of step (2), or is the product obtained by subjecting the product of step (2) to a third treatment, wherein the third treatment is one or more of an acid solution, phosphorus modification, and ammonia washing resurrection treatment.

14. The method for resurrecting spent catalytic cracking catalyst according to claim 1, characterized in that: The nickel content of the first spent catalyst is 0-0.8 wt % in terms of NiO.

15. The method for resurrecting spent catalytic cracking catalyst according to claim 5, characterized in that: The first waste catalyst is contacted with the aluminum compound dispersion, and the temperature of the first waste catalyst is 90-200° C.; the calcination in step (S3) has a calcination time of 1-3 hours.

16. The method for resurrecting spent catalytic cracking catalyst according to claim 8, characterized in that: The heat treatment temperature is 70-90° C., and the heat treatment time is 2-5 hours or 5-24 hours.

17. The method for resurrecting spent catalytic cracking catalyst according to claim 10, characterized in that: The concentration of the ammonium fluorosilicate solution is 0.2-0.6 mol / L.

18. The method for resurrecting spent catalytic cracking catalyst according to claim 12, characterized in that: The buffer is an ammonium salt of an organic acid with a carbon number less than 4 in the molecule.

19. The method for resurrecting spent catalytic cracking catalyst according to claim 18, characterized in that: The buffer is one or more of ammonium oxalate, ammonium formate and ammonium acetate.

20. A resurrected catalyst prepared by the method according to any one of claims 1 to 19.