A modified porous carbon material and its preparation method and application
Through electrostatic treatment and carbonization treatment, the combination of polyolefin and porous carbon materials is generated, which solves the problem of volume expansion and insufficient capacity of the negative electrode material of sodium ion battery and improves the first Coulomb efficiency of sodium ion battery and electrochemical properties, the commercial application of sodium ion batteries has been realized.
Patent Information
- Application Number
- CN202310222812.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-09
AI Technical Summary
The existing sodium ion battery anode materials cannot meet commercial applications due to volume expansion and powdering problems, and the low potential platform capacity of amorphous carbon materials is insufficient, resulting in a lower first-time Coulomb for sodium ion batteries.
By mixing the electrostatically treated polyolefin with porous carbon, pre-oxidation and carbonization, the modified porous carbon material is generated, its surface structure is regulated, SEI film generation is reduced, and the first-time Coulomb efficiency and low-potential platform capacity of sodium ion batteries are improved.
As the negative electrode material of sodium ion battery, the modified porous carbon material significantly improves the first charging capacity and platform capacity, enhances the electrochemical performance, and meets the requirements of commercial applications.
Smart Images

Figure CN116062734B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a modified porous carbon material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have shown broad application prospects and potential huge economic benefits in portable electronic devices, electric vehicles, space technology, defense industry, etc. due to their advantages of light weight, high energy and power density, stable discharge, and environmental friendliness. However, limited lithium resources and the continuous increase in lithium raw material prices restrict the large-scale development of lithium-ion batteries.
[0003] The working principle of sodium-ion batteries is similar to that of lithium-ion batteries. During the charging process, sodium ions are released from one end of the positive electrode and embedded in the negative electrode material. The charging capacity is closely related to the number of embedded sodium ions, that is, the more sodium ions are embedded, the higher the charging capacity. During the discharge process, the sodium ions embedded in the negative electrode material are released and move back to the positive electrode. Therefore, the negative electrode material also determines the electrochemical performance of the sodium-ion battery. However, since the radius of sodium ions is larger than that of lithium ions, the existing graphite negative electrode material for lithium-ion batteries cannot be used as the negative electrode material for sodium-ion batteries.
[0004] At present, the negative electrode materials of sodium ion batteries mainly include amorphous carbon materials and non-carbon materials (including metal and oxide materials, alloy materials, etc.). Although non-carbon materials show high sodium storage capacity, they have problems such as volume expansion and pulverization, which cannot meet the commercial application of sodium ion batteries. Amorphous carbon materials have the advantages of abundant resources and simple preparation, but during the charging and discharging process, the electrolyte easily forms a SEI film on the negative electrode surface, resulting in a low first coulomb of the sodium ion battery; at the same time, the insufficient low potential platform capacity of amorphous carbon materials also limits their commercial application. Summary of the invention
[0005] The purpose of the present invention is to provide a modified porous carbon material and a preparation method and application thereof. The modified porous carbon material provided by the present invention is used as the negative electrode of a sodium ion battery, which can improve the first coulombic efficiency and low potential platform capacity of the sodium ion battery.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a modified porous carbon material, comprising the following steps:
[0008] The electrostatically treated polyolefin and porous carbon are mixed, and pre-oxidized and carbonized in sequence to obtain a modified porous carbon material.
[0009] Preferably, the monomers of the polyolefin include one or more of ethylene, propylene, butene, pentene, hexene and octene;
[0010] The specific surface area of the porous carbon is 800 to 3500 m 2 / g.
[0011] Preferably, the mass ratio of the polyolefin to the porous carbon is 1:0.1-2.
[0012] Preferably, the mixing method is ball milling;
[0013] The ball-to-material ratio of the ball mill is 12-40:1, the rotation speed of the ball mill is 200-600 rpm, and the time is 4-48 hours.
[0014] Preferably, the pre-oxidation temperature is 230-450° C., the heating rate to the pre-oxidation temperature is 1-10° C. / min, and the holding time is 10-240 min.
[0015] Preferably, the carbonization is carried out in a protective atmosphere.
[0016] Preferably, the carbonization temperature is 800-1500° C., the heating rate to the carbonization temperature is 1-15° C. / min, and the holding time is 30-480 min.
[0017] The present invention also provides a modified porous carbon material prepared by the preparation method described in the above technical solution.
[0018] Preferably, the specific surface area of the modified porous carbon material is less than 300 m 2 / g.
[0019] The present invention also provides the use of the modified porous carbon material described in the above technical solution as a negative electrode material for a sodium ion battery.
[0020] The present invention provides a method for preparing a modified porous carbon material, comprising the following steps: mixing electrostatically treated polyolefin and porous carbon, and sequentially performing pre-oxidation and carbonization to obtain the modified porous carbon material. In the present invention, the electrostatic treatment causes a large amount of charge to be carried on the surface of the polyolefin, and during the mixing process, the porous carbon particles can be uniformly adsorbed by electrostatic action to achieve micron-level mixing, so that the polyolefin can be carbonized in situ at the pores of the porous carbon, thereby regulating the surface structure of the porous carbon and turning the open pores of the porous carbon into closed pores; during the pre-oxidation process, the polyolefin is oxidatively decomposed into oxygen-containing macromolecular fragments, which are then captured on the porous carbon surface to prevent further decomposition; the macromolecular fragments captured on the porous carbon surface undergo a cross-linking reaction with the oxygen-containing functional groups on the porous carbon surface and are fixed in situ; in the subsequent carbonization process, the oxygen-containing groups are removed, and the macromolecular fragments are carbonized in situ. The in-situ generated carbon can regulate the surface structure of the porous carbon and coat the open pores of the porous carbon into closed pores. The modified porous carbon material provided by the present invention is used as the negative electrode of the sodium ion battery. Since the closed pores prevent the solvated sodium ions from entering the internal pores, the formation of the SEI film on the surface of the carbon material is reduced, and the first coulombic efficiency of the sodium ion battery is improved. At the same time, the method retains the developed pore structure inside the porous carbon, providing sufficient storage and transmission space for sodium ions, thereby improving the low-potential platform capacity of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a digital photo of the product obtained by mixing in Example 1;
[0022] Figure 2 This is a SEM image of the meltblown fabric of the mask in the embodiment of the present invention;
[0023] Figure 3 This is the SEM image of YP50 in the embodiment of the present invention;
[0024] Figure 4 is a SEM image of the product obtained by ball milling in Example 1;
[0025] Figure 5 is a SEM image of the product obtained after pre-oxidation in Example 1;
[0026] Figure 6 This is a SEM image of the modified porous carbon material obtained in Example 1;
[0027] Figure 7 1 are nitrogen adsorption-desorption curves of the modified porous carbon materials obtained in Example 1 and Comparative Example 1;
[0028] Figure 8 The first three charge-discharge curves of a sodium ion battery obtained by using the modified porous carbon material obtained in Example 1 as the negative electrode material;
[0029] Fig. 9The first three charge-discharge curves of a sodium ion battery obtained by using the modified porous carbon material obtained in Comparative Example 1 as the negative electrode material;
[0030] Fig.10 This is the rate performance curve of the sodium ion battery obtained by using the modified porous carbon material obtained in Example 1 as the negative electrode material. DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing a modified porous carbon material, comprising the following steps:
[0032] The electrostatically treated polyolefin and porous carbon are mixed, and pre-oxidized and carbonized in sequence to obtain the modified porous carbon material.
[0033] In the present invention, unless otherwise specified, all raw materials are commercially available products well known to those skilled in the art.
[0034] In the present invention, the monomers of the polyolefin preferably include one or more of ethylene, propylene, butene, pentene, hexene and octene.
[0035] The present invention has no particular limitation on the electrostatic treatment process, and the electrostatic treatment process may be performed using a process well known to those skilled in the art.
[0036] In a specific embodiment of the present invention, the electrostatically treated polyolefin is specifically an electrostatically treated mask meltblown cloth (i.e., electret treatment), an electrostatically treated polypropylene powder, an electrostatically treated disposable PE glove, an electrostatically treated polyethylene powder, or an electrostatically treated EP rubber powder. In the present invention, the mask meltblown cloth preferably includes a newly made mask meltblown cloth or a discarded mask meltblown cloth; the disposable PE gloves preferably include a newly made disposable PE glove or a discarded disposable PE glove.
[0037] When the polyolefin is a mask meltblown cloth or a disposable PE glove, the present invention also preferably includes cutting the mask meltblown cloth or the disposable PE glove; the size after cutting is preferably 1mm x 1mm to 1cm x 1cm. The present invention has no special limitation on the cutting process, and it can be used by those skilled in the art.
[0038] The present invention has no particular limitation on the type of porous carbon, and any type known to those skilled in the art may be used. In a specific embodiment of the present invention, the porous carbon preferably includes one or more of commercial porous carbon, carbon molecular sieve and biomass porous carbon; the commercial porous carbon preferably includes one or more of YP50, YP80, YEC-8A and YEC-8B.
[0039] In the present invention, the specific surface area of the porous carbon is preferably 800 to 3500 m 2 / g.
[0040] In the present invention, the mass ratio of the polyolefin to the porous carbon matrix is preferably 1:0.1-2, more preferably 1:0.3-1.5, and even more preferably 1:0.5-1.3.
[0041] In the present invention, the mixing method is preferably ball milling; the ball-to-material ratio of the ball milling is preferably 12 to 40:1, more preferably 15 to 35:1, and more preferably 20 to 30:1; the rotation speed of the ball milling is preferably 200 to 600 rpm, more preferably 250 to 550 rpm, and more preferably 300 to 500 rpm; the time is preferably 4 to 48 h, more preferably 4 to 40 h, and more preferably 4 to 35 h. In the present invention, the ball milling method is preferably dry ball milling. The present invention does not have any special limitation on the ball milling process, and the process familiar to those skilled in the art can be used. In the present invention, micron-level mixing of polyolefin and porous carbon can be achieved through the combined action of ball milling and electrostatic treatment.
[0042] In the present invention, the pre-oxidation temperature is preferably 230-450°C, more preferably 250-420°C, and more preferably 280-400°C; the heating rate to the pre-oxidation temperature is 1-10°C / min, more preferably 2-9°C / min, and more preferably 3-8°C / min; the holding time is 10-240min, more preferably 20-230min, and more preferably 30-200min. In the present invention, the pre-oxidation is preferably carried out in an air atmosphere. In the present invention, the pre-oxidation is preferably carried out in a muffle furnace. In the present invention, during the pre-oxidation process, the porous carbon can capture the macromolecular fragments produced by the oxidative decomposition of polyolefins to prevent the macromolecular fragments from further decomposing; the macromolecular fragments captured on the surface of the porous carbon undergo a cross-linking reaction with the oxygen-containing functional groups on the surface of the porous carbon and are fixed in situ; at the same time, by precisely controlling the pre-oxidation conditions, the decomposition rate and carbonization rate of the polyolefin are balanced, thereby controlling the coating amount of the polyolefin-based carbon.
[0043] After the pre-oxidation, the present invention also preferably includes cooling the obtained product to room temperature. The present invention has no particular limitation on the cooling process, and any method known to those skilled in the art can be used.
[0044] In the present invention, the carbonization temperature is preferably 800-1500°C, more preferably 900-1400°C, and more preferably 1000-1300°C; the heating rate to the carbonization temperature is 1-15°C / min, more preferably 2-14°C / min, and more preferably 5-10°C / min; the holding time is preferably 30-480min, more preferably 50-450min, and more preferably 80-400min. In the present invention, the carbonization is preferably carried out in a protective atmosphere; the protective atmosphere preferably includes one or more of nitrogen, helium and argon. In the present invention, the carbonization is preferably carried out in a tubular furnace. In the present invention, the oxygen-containing groups introduced during the pre-oxidation process can be removed by carbonization, thereby reducing the defects of the carbon material finally obtained.
[0045] The preparation method provided by the invention is simple and convenient, and can also realize the recycling and reuse of waste polyolefins.
[0046] The present invention also provides a modified porous carbon material prepared by the preparation method described in the above technical solution. In the present invention, the modified porous carbon material preferably includes porous carbon and in-situ carbon loaded on the surface of the porous carbon; the in-situ carbon is carbon formed after pre-oxidation and carbonization of polyolefin. In the present invention, the loading percentage of the in-situ carbon in the modified porous carbon material is preferably 15 to 50%.
[0047] In the present invention, the utilization rate of the polyolefin is preferably 10 to 45%. In the present invention, the utilization rate is preferably calculated according to the following formula:
[0048] Utilization rate = (mass of modified porous carbon material - mass of initial porous carbon) / mass of polyolefin.
[0049] In the present invention, the specific surface area of the modified porous carbon material is preferably less than 300 m 2 In the present invention, by mixing the electrostatically treated polyolefin and porous carbon, and then pre-oxidizing and carbonizing, carbon can be generated in situ on the porous carbon surface, and the generated carbon can regulate the surface structure of the porous carbon, so that the open pores on the porous carbon surface become closed pores.
[0050] The present invention also provides the use of the modified porous carbon material described in the above technical solution as a negative electrode material for a sodium ion battery. The present invention has no special limitation on the specific implementation of the application, and any method known to those skilled in the art can be used.
[0051] In order to further illustrate the present invention, a modified porous carbon material provided by the present invention and its preparation method and application are described in detail below in combination with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0052] Example 1
[0053] 1 g of shredded discarded mask meltblown cloth (treated with electret, with a size of 0.5 cm x 0.5 cm) and 0.4 g of YP50 were mixed and ball-milled. The conditions during the ball-milling process were: ball-to-material ratio of 30:1, rotation speed of 400 rpm, and time of 5 h.
[0054] The obtained mixture (as shown in the figure) Figure 1 The obtained carbonized porous carbon material was prepared by heating to 300°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, keeping the temperature for 1 hour, and cooling to room temperature; the carbonized carbon material was prepared by heating to 1300°C at a heating rate of 5°C / min in an argon atmosphere for 2 hours to obtain 0.537 g of modified porous carbon material (the loading amount of in-situ carbon was 34.3%, and the utilization rate of the mask was 13.7%).
[0055] Example 2
[0056] 1 g of electrostatically treated polypropylene powder (size 300 mesh) and 0.8 g of YP50 were mixed and ball-milled. The conditions during the ball-milling process were: ball-to-material ratio of 30:1, rotation speed of 400 rpm, and time of 5 h.
[0057] The obtained mixture was placed in a muffle furnace, heated to 330°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, and kept warm for 1 hour; then, the mixture was carbonized at a heating rate of 5°C / min in an argon atmosphere, and kept warm for 2 hours to obtain 1.0 g of modified porous carbon material (the loading amount of in-situ carbon was 25.4%, and the utilization rate of polypropylene powder was 20.3%).
[0058] Example 3
[0059] 1 g of shredded electrostatically treated discarded disposable PE gloves (size 0.5 cm x 0.5 cm) and 0.5 g of YP50 were mixed and ball-milled. The parameters of the ball-to-material ratio were 30:1, the rotation speed was 400 rpm, and the time was 5 h.
[0060] The obtained mixture was placed in a muffle furnace, heated to 330°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, and kept warm for 1 hour; then, the mixture was carbonized at a heating rate of 5°C / min in an argon atmosphere, and kept warm for 2 hours to obtain 0.683 g of modified porous carbon material (the loading amount of in-situ carbon was 36.7%, and the utilization rate of disposable gloves was 18.3%).
[0061] Example 4
[0062] 1 g of electrostatically treated polyethylene powder (300 mesh) and 0.6 g of YP50 were mixed and ball-milled. The parameters of the ball-to-material ratio were 30:1, the rotation speed was 400 rpm, and the time was 5 h.
[0063] The obtained mixture was placed in a muffle furnace, heated to 350°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, and kept warm for 1 hour; then, the mixture was carbonized at a heating rate of 5°C / min in an argon atmosphere, and kept warm for 2 hours to obtain 0.827 g of modified porous carbon material (the in-situ carbon loading was 37.9%, and the utilization rate of polyethylene was 22.7%).
[0064] Example 5
[0065] 1 g of shredded discarded mask meltblown cloth (after electret treatment, size 0.5 cm x 0.5 cm) and 0.4 g of YP80 were mixed and ball milled. The conditions during the ball milling process were: ball-to-material ratio of 30:1, rotation speed of 400 rpm, and time of 5 h.
[0066] The obtained mixture was placed in a muffle furnace, heated to 330°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, and kept warm for 1 hour; then, the mixture was carbonized at a heating rate of 5°C / min in an argon atmosphere, and kept warm for 2 hours to obtain 0.540g of modified porous carbon material (wherein the in-situ carbon loading was 35.0%, and the utilization rate of the mask was 14.0%).
[0067] Example 6
[0068] 1 g of electrostatically treated EPDM powder (300 mesh) and 0.4 g of YP50 were mixed and ball-milled. The parameters of the ball-to-material ratio were 30:1, the rotation speed was 400 rpm, and the time was 5 h.
[0069] The obtained mixture was placed in a muffle furnace, heated to 330°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, and kept warm for 1 hour; then, the mixture was carbonized at a heating rate of 5°C / min in an argon atmosphere, and kept warm for 2 hours to obtain 0.540g of modified porous carbon material (wherein the in-situ carbon loading was 35.0%, and the utilization rate of EPDM rubber was 14.0%).
[0070] Comparative Example 1
[0071] 0.2 g of YP50 was placed in a muffle furnace, and the temperature was raised to 330°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, and kept warm for 1 hour; then, the temperature was raised to 1300°C at a heating rate of 5°C / min in an argon atmosphere for carbonization, and kept warm for 2 hours to obtain a porous carbon material.
[0072] Comparative Example 2
[0073] 1 g of shredded discarded mask meltblown cloth (after electret treatment, size 0.5 cm x 0.5 cm) and 0.8 g of YP50 were mixed and ball milled. The conditions and parameters during the ball milling process were: ball-to-material ratio of 30:1, rotation speed of 400 rpm, and time of 5 h.
[0074] The obtained mixture was carbonized at 1300°C at a heating rate of 5°C / min under an argon atmosphere and kept warm for 2 hours to obtain a porous carbon material (wherein the loading amount of in-situ carbon was 0 and the utilization rate of the mask was 0).
[0075] Comparative Example 3
[0076] 1 g of shredded discarded mask meltblown fabric (after electret treatment, size 0.5 cm x 0.5 cm) was ball milled. The conditions and parameters during the ball milling process were: ball-to-material ratio of 30:1, rotation speed of 400 rpm, and time of 5 h;
[0077] The ball-milled discarded mask meltblown cloth was placed in a muffle furnace, and pre-oxidized at a heating rate of 5°C / min in an air atmosphere at 330°C, and kept warm for 1 hour; then, carbonized at a heating rate of 5°C / min in an argon atmosphere at 1300°C, and kept warm for 2 hours, but no carbon material was obtained.
[0078] Performance Testing
[0079] Test Example 1
[0080] The discarded mask meltblown cloth and YP50 in the examples and the ball milling product, pre-oxidation product and modified porous carbon material in Example 1 were subjected to scanning electron microscopy tests, and the test images obtained were as follows: Figures 2 to 6 As shown, Figure 2 For masks, Figure 3 YP50, Figure 4 For ball milling products, Figure 5 As the pre-oxidation product, Figure 6 To modify porous carbon materials, according to Figures 2 to 6 It can be seen that after ball milling, YP50 is evenly distributed on the surface of the mask fiber, after pre-oxidation, the mask fragments are coated on the porous carbon surface, and after carbonization, the mask fragments are carbonized in situ and attached to the surface of the porous carbon.
[0081] Test Example 2
[0082] The modified porous carbon materials obtained in Example 1 and Comparative Example 1 were tested for specific surface area, and the nitrogen adsorption-desorption curves obtained were as follows: Figure 7 As shown, from Figure 7 It can be seen that the specific surface area of the modified porous carbon material obtained in Example 1 is 260.03 m2 / g, the specific surface area of the porous carbon material obtained in Comparative Example 1 is 1656.73m 2 / g.
[0083] Test Example 3
[0084] The modified porous carbon materials obtained in Examples 1 to 6 and Comparative Example 1 were used as negative electrode materials for sodium ion batteries to test their electrochemical properties;
[0085] The test method is:
[0086] The modified porous carbon material and sodium carboxymethyl cellulose were mixed in a mass ratio of 95:5, and then ground into a slurry by adding an appropriate amount of water. The obtained slurry was evenly scraped onto the current collector copper foil, dried, and cut into a circular electrode with a diameter of 10 mm; the circular electrode was dried at 120° C. under vacuum conditions for 10 h and then transferred to a glove box; in an Ar atmosphere, sodium metal was used as a counter electrode, and 1 mol of NaClO4 was dissolved in 1 L of a solution of ethylene carbonate and diethyl carbonate in a volume ratio of 1:1 was used as an electrolyte to assemble the battery to obtain a CR2025 button battery;
[0087] The obtained CR2025 button battery was subjected to charge and discharge tests, and the test conditions were: charge and discharge rate was 0.1C, discharge cut-off voltage was 0.001V, and charge cut-off voltage was 2.5V;
[0088] The test results are shown in Table 1;
[0089] Table 1 Electrochemical performance of sodium ion batteries using modified porous carbon materials obtained in Examples 1 to 6 and Comparative Example 1 as negative electrode materials
[0090] <![CDATA[Initial charge capacity / mAh·g -1 > <![CDATA[Platform capacity / mAhg -1 > First coulombic efficiency / % Example 1 333.2 228.3 88.0 Example 2 330.2 225.4 88.8 Example 3 327.6 223.1 85.1 Example 4 315.9 227.0 85.6 Example 5 314.5 221.3 87.9 Example 6 294.4 212.4 85.0 Comparative Example 1 101.8 0.0 19.4
[0091] It can be seen from Table 1 that when the modified porous carbon material provided by the present invention is used as the negative electrode of the sodium ion battery, the first charge capacity, platform capacity and first cycle coulombic efficiency are significantly improved compared with the unmodified porous carbon.
[0092] The first three charge-discharge curves of a sodium ion battery prepared by using the modified porous carbon material obtained in Example 1 as the negative electrode material are as follows: Figure 8 As shown, from Figure 8 It can be seen that the modified porous carbon material provided by the present invention exhibits a relatively long platform capacity when used as the negative electrode of a sodium ion battery.
[0093] The first three charge-discharge curves of a sodium ion battery prepared by using the porous carbon material obtained in Comparative Example 1 as the negative electrode material are as follows: Fig. 9 As shown, from Fig. 9It can be seen that when unmodified porous carbon materials are used as negative electrode materials for sodium ion batteries, they not only have no platform capacity, but also have extremely low initial efficiency and cannot be put into practical use.
[0094] Test Example 4
[0095] The modified porous carbon material obtained in Example 1 was used as the negative electrode material, and a button battery was assembled in the manner of Test Example 3. The rate performance of the obtained button battery was tested under the following test conditions: the charge and discharge rates were 0.1C, 0.2C, 0.5C, 1C and 2C, respectively, the discharge cut-off voltage was 0.001V, and the charge cut-off voltage was 2.5V;
[0096] The obtained rate performance curve is as follows: Fig.10 As shown, from Fig.10 It can be seen that the modified porous carbon material has good rate performance.
[0097] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a modified porous carbon material, It is characterized in that The steps are: 1 g of shredded electret treated discarded mask meltblown cloth with a size of 0.5 cm × 0.5 cm was mixed with 0.4 g of YP50 and ball milled. The conditions during the ball milling process were: ball-to-material ratio of 30:1, rotation speed of 400 rpm, and time of 5 h. The obtained mixture was placed in a muffle furnace, heated to 300°C at a heating rate of 5°C / min in an air atmosphere for pre-oxidation, kept warm for 1 hour, and cooled to room temperature; then, the mixture was heated to 1300°C at a heating rate of 5°C / min in an argon atmosphere for carbonization, kept warm for 2 hours, and 0.537g of modified porous carbon material was obtained, of which the in-situ carbon loading was 34.3% and the utilization rate of the mask was 13.7%.