High-pressure polyethylene for fruit net bag and its preparation method and application
By using high-pressure polyethylene and its preparation method in the production of fruit net bags, the problem of lack of special foaming resin in China has been solved. The high-pressure polyethylene produced has high elongation at break and low density, which is suitable for the production of fruit net bags and has achieved Efficient production with low energy consumption.
Patent Information
- Application Number
- CN202111276392.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-29
AI Technical Summary
There is a lack of low-density polyethylene foaming resin for fruit net bags in China, and the market generally uses general-purpose foaming materials, resulting in low foaming ratio and poor resilience.
Provide high-pressure polyethylene for fruit net bags and its preparation method. By performing polymerization reaction under the initiator system of regulator and organic peroxide, controlling the polymerization temperature and pressure, high-pressure polyethylene with narrow molecular weight distribution is produced, which is suitable for foamed net bags. Production.
High-pressure polyethylene with high elongation at break is suitable for the production of fruit net bags. It has high melt index and low density, simple reaction, low energy consumption, and a single-pass conversion rate of 22 to 25%.
Smart Images

Figure BDA0003330051690000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer synthesis, in particular to high-pressure polyethylene used for fruit net bags and a preparation method and application thereof. Background Art
[0002] Low-density polyethylene is suitable for various molding processes of thermoplastics. For example, it can be used for film products, injection molding products, extrusion foam products, and can also be used as a masterbatch carrier resin. Polyethylene foam products have good physical and chemical properties, and are gradually becoming a variety with diverse products, large production volume, and wide application. And because polyethylene has a light capacity, low thermal conductivity, and a wide range of sound insulation, heat insulation, and buffering physical properties, polyethylene foam materials have developed rapidly in recent years. They are mainly used in the production of coils and sheets for shoes, as well as air conditioning insulation, heterosexual packaging, children's toys, sports goods, etc., and are deeply loved by manufacturers.
[0003] In recent years, with the improvement of people's living standards, the use of fruit nets has increased year by year. Fruits suitable for plastic nets include apples, oranges, tangerines, persimmons, watermelons, etc. Polyethylene foam materials are non-toxic and can be in contact with food, so they can be used as raw materials for fruit nets. However, there is no low-density polyethylene foam resin specifically for fruit nets in China. The market generally uses general materials for foaming, which has the disadvantages of low foaming ratio and poor resilience. Summary of the invention
[0004] In view of this, the purpose of the present invention is to address the shortcomings of the prior art and provide high-pressure polyethylene for fruit net bags and a preparation method and application thereof. The preparation method of the present invention is simple, easy to operate, and has low energy consumption. The prepared high-pressure polyethylene has a narrow molecular weight distribution and a high elongation at break, and is suitable for the production of foam net bags.
[0005] The objectives of the present invention are achieved through the following technical solutions.
[0006] In a first aspect, the present invention provides a method for preparing high-pressure polyethylene for fruit net bags, wherein the preparation method comprises the following steps:
[0007] S100, subjecting ethylene to a first polymerization reaction in the presence of a regulator and a first organic peroxide initiation system to obtain a first polymerization product containing unreacted ethylene, wherein the first organic peroxide initiation system comprises tert-butyl peroxypivalate and tert-butyl peroxy-2-ethylhexanoate, and the temperature of the first polymerization reaction is 320-340° C. and the pressure is 250-260 MPa;
[0008] S200, subjecting the first polymerization product containing unreacted ethylene to a second polymerization reaction in the presence of a second organic peroxide initiation system to obtain a second polymerization product, wherein the second organic peroxide initiation system comprises acetic peroxide, di-tert-butyl hydroperoxide and p-menthane hydroperoxide, and the temperature of the second polymerization reaction is 331-335° C. and the pressure is 240-255 MPa;
[0009] S300, the second polymerization product is depressurized, separated and granulated to obtain high-pressure polyethylene.
[0010] In the present invention, the melt index of the high-pressure polyethylene can be adjusted by using an adjusting agent.
[0011] According to the preparation method provided by the present invention, wherein the regulator in step S100 is C2-C6 alkane, preferably propane.
[0012] In some embodiments, in step S100, the amount of the regulator used is 150±25 ppm based on the weight of the added ethylene.
[0013] According to the preparation method provided by the present invention, in step S100, the first organic peroxide initiation system is added in the form of a solution, and the solvent in the solution of the first organic peroxide initiation system is preferably solvent oil A. Examples of solvent oil A suitable for use in the present invention include, but are not limited to, isoundecane, isododecane, and n-dodecane. In some embodiments, the solvent oil A is selected from at least one of isoundecane and isododecane.
[0014] According to the preparation method provided by the present invention, in step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5-0.75% by weight, preferably 0.5-0.65% by weight, and more preferably 0.5-0.6% by weight; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.87-1.2% by weight, preferably 0.95-1.2% by weight, and more preferably 0.95-1.0% by weight.
[0015] According to the preparation method provided by the present invention, the time of the first polymerization reaction in step S100 is 8 to 9 seconds.
[0016] According to the preparation method provided by the present invention, the first polymerization reaction in step S100 is carried out in the presence of air. In some embodiments, based on the high-pressure polyethylene output of 22.8 t / h, the amount of air used in step S100 is 4 to 8 m 3 / h.
[0017] According to the preparation method provided by the present invention, step S100 comprises:
[0018] S101, mixing ethylene with flash ethylene from a primary compressor and / or a secondary compressor, compressing the ethylene to 250-260 MPa via a primary compressor, mixing the ethylene with the circulating material and entering a secondary compressor to be compressed to 265-270 MPa, and adding the regulator from the inlet of the primary compressor;
[0019] S102, sending the mixed gas flow compressed to 265-270 MPa by the secondary compressor into the first reactor, preheating the first reactor, adding the first organic peroxide initiation system from the first initiator injection port, adding air from the inlet of the secondary compressor, heating to 320-340° C., preferably 330-340° C., and conducting a first polymerization reaction at a pressure of 250-260 MPa, preferably 250-255 MPa.
[0020] In some embodiments, in step S102, the first reactor is preheated to 120-160°C, for example, 140°C.
[0021] According to the preparation method provided by the present invention, in step S200, the second organic peroxide initiation system is added in the form of a solution, and the solvent in the solution of the second organic peroxide initiation system is preferably solvent oil B. Examples of solvent oil B suitable for use in the present invention include, but are not limited to, isoundecane, isododecane, isododecane and n-dodecane.
[0022] In some embodiments, based on the weight of the first polymerization reaction product, the amount of acetic acid peroxide in the second organic peroxide initiation system is 0.4 to 0.6 weight %, preferably 0.5 to 0.56 weight %; the amount of di-tert-butyl hydroperoxide is 0.8 to 1.2 weight %, preferably 0.9 to 1.0 weight %; the amount of menthane hydrogen peroxide is 0.4 to 0.6 weight %, preferably 0.5 to 0.6 weight %.
[0023] According to the preparation method provided by the present invention, the time of the second polymerization reaction in step S200 is 13 to 15 seconds.
[0024] According to the preparation method provided by the present invention, step S200 comprises:
[0025] S201, sending the first polymerization product containing unreacted ethylene into the second reactor, adding the second organic peroxide initiation system from the second initiator injection port, and carrying out the second polymerization reaction at a temperature of 331-335° C. and a pressure of 240-250 MPa.
[0026] According to the preparation method provided by the present invention, step S200 further comprises: before step S201, cooling the first polymerization product containing unreacted ethylene, preferably cooling to 30-45°C.
[0027] According to the preparation method provided by the present invention, step S300 comprises:
[0028] S301, the second polymerization product is cooled to 30-45° C. in the second reactor, the pressure is reduced by the discharge valve at the outlet, and the product is discharged into a high-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product;
[0029] S302, melting the polyethylene product obtained in step S301, and sending it into a low-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product, and granulating them to obtain high-pressure polyethylene.
[0030] According to the preparation method provided by the present invention, the single-pass conversion rate of the preparation method of the present invention is generally 22-25%.
[0031] According to the preparation method provided by the present invention, the method further comprises sending the ethylene gas from the high-pressure separator and / or the low-pressure separator to step S101 as a circulating material.
[0032] According to the preparation method provided by the present invention, a tubular high-pressure polymerization process device is used to implement the preparation method of the present invention. The present invention has no special limitation on the tubular high-pressure polymerization process device, and any tubular high-pressure polymerization process device known in the art can be used.
[0033] In a second aspect, the present invention also provides high-pressure polyethylene produced by the above preparation method.
[0034] According to the high-pressure polyethylene provided by the present invention, as measured according to GB / T 3682.1-2000, the melt index of the high-pressure polyethylene at a temperature of 190°C and a load of 2.16Kg is 4 to 10g / 10min, preferably 5 to 8g / 10min; and / or the density of the high-pressure polyethylene is 0.916 to 0.924g / cm 3 , preferably 0.918~0.922g / cm 3 ; The molecular weight distribution index (Mw / Mn) of the high-pressure polyethylene is 4 to 9, preferably 5 to 6.
[0035] According to the high-pressure polyethylene provided by the present invention, the tensile strength of the high-pressure polyethylene is greater than 10 MPa, preferably greater than 11 MPa; the tensile fracture strain is greater than 300%, preferably greater than 450%.
[0036] In a third aspect, the present invention also provides the use of the high-pressure polyethylene in the preparation of a foam net bag.
[0037] The present invention has the following advantages:
[0038] (1) In the present invention, high-pressure polyethylene is prepared by adjusting the polymerization process, especially the selection of the initiator system, the control of the polymerization pressure and the polymerization temperature, and further controlling the selection and addition amount of the regulator as needed, which is of great significance for the research and development of polyethylene special materials;
[0039] (2) The method of the present invention is simple, easy to operate, and has low energy consumption. The single-pass conversion rate of the reaction is 22-25%. The high-pressure polyethylene produced has a narrow molecular weight distribution and a high elongation at break, and is suitable for the production of foamed net bags. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.
[0041] Example 1
[0042] (1) Ethylene is mixed with flash ethylene from the primary compressor and the secondary compressor, compressed to 255 MPa by the primary compressor, mixed with the circulating material and enter the inlet of the secondary compressor. The amount of propane as a regulator is 150 ppm based on the weight of the added ethylene, and added from the inlet tank of the primary compressor to obtain a mixed gas flow.
[0043] (2) The secondary compressor compresses the mixed gas flow to 269.1 MPa, and then enters the front part of the first reactor. The first reactor is preheated to 140° C., and the isonadecane solution of the first organic peroxide initiation system is injected from the first initiator injection port, wherein the amount of tert-butyl peroxy pivalate is 0.5% by weight, and the amount of tert-butyl peroxy-2-ethylhexanoate initiator is 0.95% by weight based on the weight of the added ethylene; the amount of hexene added is 100m 3 / h, the temperature of air added from the inlet of the secondary compressor is raised to 330°C, and the first polymerization reaction is carried out at a pressure of 225 MPa. The reaction time is 8 to 9 seconds to obtain a first polymerization reaction product containing unreacted ethylene.
[0044] (3) The first polymerization product containing unreacted ethylene is cooled to 60° C. and fed into a second reactor, and an isoundecane solution of a second organic peroxide initiation system is added from a second initiator injection port, wherein, based on the weight of the first polymerization product, the amount of acetic peroxide is 0.5% by weight, the amount of di-tert-butyl hydroperoxide is 0.9% by weight, and the amount of p-menthane hydroperoxide is 0.5% by weight. The reaction is reinitiated to carry out a second polymerization reaction to obtain a second polymerization product. The reaction temperature is 331° C., the pressure is 240 MPa, and the reaction time is 13 to 15 seconds.
[0045] (4)) The second polymerization product is cooled to 70°C in the second reactor and the pressure is reduced by the discharge valve at the outlet. The product is discharged into a high-pressure separator for gas and material separation to obtain ethylene gas and polyethylene product. The polyethylene product is melted and sent to a low-pressure separator for gas and material separation to obtain ethylene gas and polyethylene product, which are then granulated to obtain high-pressure polyethylene.
[0046] The single-pass conversion rate of the preparation method of Example 1 is generally 24.3%. The ethylene gas from the high-pressure separator and the low-pressure separator is sent to step (1) as a circulating material.
[0047] Example 2
[0048] The high pressure polyethylene was prepared by the same method as in Example 1, except that:
[0049] (a) The amount of propane used as the regulator in step (1) is 165 ppm.
[0050] (b) In step (2), the amount of tert-butyl peroxy pivalate is 0.6% by weight, the amount of tert-butyl peroxy-2-ethylhexanoate initiator is 0.99% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 340° C., pressure is 260 MPa, and reaction time is 8 to 9 seconds.
[0051] (c) In step (3), the amount of acetic peroxide is 0.56% by weight, the amount of di-tert-butyl hydroperoxide is 0.98% by weight, the amount of para-menthane hydroperoxide is 0.45% by weight, and the conditions of the second polymerization reaction are as follows: temperature is 331° C., pressure is 245 MPa, and reaction time is 13 to 15 seconds.
[0052] The single-pass conversion rate of the preparation method of Example 2 is generally 24.6%.
[0053] Example 3
[0054] The high pressure polyethylene was prepared by the same method as in Example 1, except that:
[0055] (a) The amount of propane used as the regulator in step (1) is 140 ppm.
[0056] (b) In step (2), the amount of the organic peroxide tert-butyl peroxy pivalate is 0.62% by weight, the amount of the tert-butyl peroxy-2-ethylhexanoate initiator is 1.2% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 330° C., pressure is 260 MPa, and reaction time is 8 to 9 seconds.
[0057] (c) In step (3), the amount of acetic peroxide is 0.53% by weight, the amount of di-tert-butyl hydroperoxide is 0.98% by weight, the amount of p-menthane hydroperoxide is 0.60% by weight, and the conditions of the second polymerization reaction are as follows: temperature is 335° C., pressure is 245 MPa, and reaction time is 13 to 15 seconds.
[0058] The single-pass conversion rate of the preparation method of Example 3 is generally 24.8%.
[0059] Example 4
[0060] The high pressure polyethylene was prepared by the same method as in Example 1, except that:
[0061] (a) The amount of propane used as the regulator in step (1) is 135 ppm.
[0062] (b) In step (2), the amount of the organic peroxide tert-butyl peroxy pivalate is 0.57% by weight, the amount of the tert-butyl peroxy-2-ethylhexanoate initiator is 1.0% by weight, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 330° C., pressure is 260 MPa, and reaction time is 8 to 9 seconds.
[0063] (c) In step (3), the amount of acetic peroxide is 0.55 wt %, the amount of di-tert-butyl hydroperoxide is 1.0 wt %, the amount of para-menthane hydroperoxide is 0.60 wt %, and the conditions of the second polymerization reaction are as follows: temperature is 335° C., pressure is 245 MPa, and reaction time is 13 to 15 seconds.
[0064] The single-pass conversion rate of the preparation method of Example 4 is generally 23.9%.
[0065] Example 5
[0066] The high pressure polyethylene was prepared by the same method as in Example 1, except that:
[0067] (a) The amount of propane used as the regulator in step (1) is 158 ppm.
[0068] (b) In step (2), the amount of the organic peroxide tert-butyl peroxypivalate is 0.6 wt %, the amount of tert-butyl peroxy-2-ethylhexanoate is 0.96 wt %, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature is 330° C., pressure is 250 MPa, and reaction time is 8-9 seconds.
[0069] (c) In step (3), the amount of acetic peroxide is 0.55 wt %, the amount of di-tert-butyl hydroperoxide is 1.0 wt %, the amount of para-menthane hydroperoxide is 0.60 wt %, and the conditions of the second polymerization reaction are as follows: temperature is 333° C., pressure is 255 MPa, and reaction time is 13 to 15 seconds.
[0070] The single-pass conversion rate of the preparation method of Example 5 is generally 24.4%.
[0071] Example 6
[0072] The high pressure polyethylene was prepared by the same method as in Example 1, except that:
[0073] (a) The amount of propane used as the regulator in step (1) is 175 ppm.
[0074] (b) in step (2), the amount of the organic peroxide tert-butyl peroxypivalate is 0.65 wt %, the amount of tert-butyl peroxy-2-ethylhexanoate is 0.96 wt %, and air is added from the inlet of the secondary compressor. The conditions of the first polymerization reaction are as follows: temperature 330° C., pressure 250 MPa, and reaction time 8-9 seconds.
[0075] (c) In step (3), the amount of acetic peroxide is 0.55 wt %, the amount of di-tert-butyl hydroperoxide is 1.0 wt %, the amount of para-menthane hydroperoxide is 0.60 wt %, and the conditions of the second polymerization reaction are as follows: reaction temperature is 333° C., pressure is 255 MPa, and reaction time is 13 to 15 seconds.
[0076] The single-pass conversion rate of the preparation method of Example 6 is generally 24.7%.
[0077] Performance Testing
[0078] In the present invention, the following test standards and methods are used to test high pressure polyethylene.
[0079] Melt mass flow rate: measured according to GB / T 3682.1-2000, conditions: 190°C, 2.16Kg; unit: g / 10min.
[0080] Density: measured according to GB / T 1033.2-2010, condition: temperature 23℃; unit: kg / m 3.
[0081] Tensile yield strength: measured according to ASTM D638-2010, unit, MPa.
[0082] Elongation at break: measured according to ASTM D638-2010, %.
[0083] Molecular weight distribution (Mw / Mn): Gel permeation chromatography was used, the solvent and mobile phase were 1,2,4-trichlorobenzene (containing 0.025 wt% antioxidant 2,6-dibutyl-p-cresol), the column temperature was 150°C, the flow rate was 1.0 ml / min, and narrow distribution polystyrene standards were used for universal calibration.
[0084] The properties of the high pressure polyethylene prepared in Examples 1 to 6 are shown in Table 1.
[0085] Table 1 Properties of high pressure polyethylene prepared in Examples 1 to 6
[0086]
[0087] As can be seen from Table 1, the high-pressure polyethylene injection molding compound prepared by the preparation method of the present invention has a narrow molecular weight distribution, a high melt index and a low density, and is suitable for the production of injection molding compounds.
[0088] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. Application of high pressure polyethylene in the preparation of foamed net bags, wherein: The method for preparing high-pressure polyethylene comprises the following steps: S100, subjecting ethylene to a first polymerization reaction in the presence of a regulator and a first organic peroxide initiation system to obtain a first polymerization product containing unreacted ethylene, wherein the first organic peroxide initiation system comprises tert-butyl peroxypivalate and tert-butyl peroxy-2-ethylhexanoate, and the temperature of the first polymerization reaction is 320-340° C. and the pressure is 250-260 MPa; S200, subjecting the first polymerization product containing unreacted ethylene to a second polymerization reaction in the presence of a second organic peroxide initiation system to obtain a second polymerization product, wherein the second organic peroxide initiation system comprises acetic peroxide, di-tert-butyl hydroperoxide and p-menthane hydroperoxide, and the temperature of the second polymerization reaction is 331-335° C. and the pressure is 240-255 MPa; S300, the second polymerization product is subjected to pressure reduction, separation and granulation to obtain high-pressure polyethylene; The regulator in step S100 is propane; In step S100, the amount of the regulator used is 150±25 ppm based on the weight of the added ethylene.
2. The use according to claim 1, characterized in that: In step S100, the first organic peroxide initiation system is added in the form of a solution.
3. The use according to claim 2, characterized in that: In step S100, the solvent in the solution of the first organic peroxide initiation system is solvent oil A, and the solvent oil A is selected from at least one of isoundecane, isododecane and n-dodecane.
4. The use according to claim 3, characterized in that: The solvent oil A is selected from at least one of isoundecane and isododecane.
5. The use according to claim 1, characterized in that: In step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5-0.75 wt %; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.87-1.2 wt %.
6. The use according to claim 5, characterized in that: In step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5-0.65 wt %; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.95-1.2 wt %.
7. The use according to claim 6, characterized in that: In step S100, based on the weight of the added ethylene, the amount of tert-butyl peroxypivalate in the first organic peroxide initiation system is 0.5-0.6 wt %; the amount of tert-butyl peroxy-2-ethylhexanoate is 0.95-1.0 wt %.
8. The use according to any one of claims 1 to 7, characterized in that The time of the first polymerization reaction in step S100 is 8 to 9 seconds; and / or, In step S100, the first polymerization reaction is carried out in the presence of air. The high-pressure polyethylene output is 22.8 t / h, and the amount of hexene added is 100 m 3 / h, the amount of air used in step S100 is 4 to 8m 3 / h.
9. The use according to any one of claims 1 to 7, characterized in that Step S100 includes: S101, mixing ethylene with flash ethylene from a primary compressor and / or a secondary compressor, compressing the ethylene to 250-260 MPa via a primary compressor, mixing the ethylene with the circulating material and entering a secondary compressor to be compressed to 265-270 MPa, and adding the regulator from the inlet of the primary compressor; S102, sending the mixed gas flow compressed to 265-270 MPa by the secondary compressor into the first reactor, preheating the first reactor, adding the first organic peroxide initiation system from the first initiator injection port, adding air from the inlet of the secondary compressor, raising the temperature to 320-340° C., and conducting the first polymerization reaction at a pressure of 250-260 MPa.
10. The use according to claim 9, characterized in that: S102, sending the mixed gas flow compressed to 265-270 MPa by the secondary compressor into the first reactor, preheating the first reactor, adding the first organic peroxide initiation system from the first initiator injection port, adding air from the inlet of the secondary compressor, raising the temperature to 330-340° C., and conducting the first polymerization reaction at a pressure of 250-255 MPa.
11. The use according to any one of claims 1 to 7, characterized in that In step S200, the second organic peroxide initiation system is added in the form of a solution.
12. The use according to claim 11, characterized in that: The solvent in the solution of the second organic peroxide initiation system in step S200 is solvent oil B, and the solvent oil B is selected from at least one of isoundecane, isododecane and n-dodecane.
13. The use according to claim 11, characterized in that: Based on the weight of the first polymerization product, the amount of acetic acid peroxide in the second organic peroxide initiation system is 0.4-0.6 weight %; the amount of di-tert-butyl hydroperoxide is 0.8-1.2 weight %; and the amount of para-menthane hydroperoxide is 0.4-0.6 weight %.
14. The use according to claim 13, characterized in that Based on the weight of the first polymerization product, the amount of acetic acid peroxide in the second organic peroxide initiation system is 0.5-0.56 weight %; the amount of di-tert-butyl hydroperoxide is 0.9-1.0 weight %; and the amount of para-menthane hydroperoxide is 0.5-0.6 weight %.
15. The use according to any one of claims 1 to 7, characterized in that Step S200 includes: S201, sending the first polymerization product containing unreacted ethylene into the second reactor, adding the second organic peroxide initiation system from the second initiator injection port, and carrying out the second polymerization reaction at a temperature of 331-335° C. and a pressure of 240-250 MPa.
16. The use according to claim 15, characterized in that Step S200 further includes: before step S201, cooling the first polymerization product containing unreacted ethylene.
17. The use according to claim 16, characterized in that Cool to 30-45℃.
18. The use according to claim 15, characterized in that: The duration of the second polymerization reaction in step S200 is 13 to 15 seconds.
19. The use according to any one of claims 1 to 7, characterized in that Step S300 includes: S301, the second polymerization product is cooled to 30-45° C. in the second reactor; the pressure is reduced by the discharge valve at the outlet, and the product is discharged into a high-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product; S302, melting the polyethylene product obtained in step S301, and sending it into a low-pressure separator to separate the gas from the product material to obtain ethylene gas and polyethylene product, and granulating them to obtain high-pressure polyethylene.
20. The use according to any one of claims 1 to 7, characterized in that The melt index of the high-pressure polyethylene at a temperature of 190° C. and a load of 2.16 kg is 4 to 10 g / 10 min as measured according to GB / T 3682.1-2000; and / or the density of the high-pressure polyethylene is 0.916 to 0.924 g / cm 3 ; The molecular weight distribution index (Mw / Mn) of the high-pressure polyethylene is 4 to 9.
21. The use according to claim 20, characterized in that The melt index of the high-pressure polyethylene at a temperature of 190° C. and a load of 2.16 kg is 5 to 8 g / 10 min as measured according to GB / T 3682.1-2000; and / or the density of the high-pressure polyethylene is 0.918 to 0.922 g / cm 3 ; The molecular weight distribution index (Mw / Mn) of the high-pressure polyethylene is 5 to 6.