Low-temperature preparation method and application of metal oxide two-dimensional catalyst

By using water-soluble starch templates to prepare metal oxide two-dimensional catalysts, the problems of low activity of traditional catalysts and complex preparation processes are solved, and efficient carbon dioxide conversion and high-purity carbon monoxide production are achieved, which is suitable for industrial applications.

CN116078387BActive Publication Date: 2024-10-08HEBEI UNIVERSITY
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310144601.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2024-10-08
Estimated Expiration
2043-02-21

AI Technical Summary

Technical Problem

Traditional reverse water gas shift reaction catalysts have low activity, poor selectivity, and cumbersome preparation processes, which do not meet the needs of industrialization and are difficult to achieve efficient carbon dioxide conversion and high-purity production of carbon monoxide.

Method used

Using water-soluble starch as a template, a metal oxide two-dimensional catalyst was prepared through freeze-drying technology, and then slowly annealed at low temperature to obtain a nanosheet catalyst, which can be used in reverse water gas shift reaction to improve catalytic efficiency and selectivity.

Benefits of technology

It achieves efficient catalytic conversion of carbon dioxide, improves the purity of carbon monoxide and the stability of the catalyst, reduces the preparation temperature and equipment costs, and is suitable for industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116078387B_ABST
    Figure CN116078387B_ABST
Patent Text Reader

Abstract

The present invention provides a low-temperature preparation method and application of a metal oxide two-dimensional catalyst. The present invention uses water-soluble starch as a template and a metal salt as a precursor to form uniform two-dimensional nanosheets through freeze-drying technology and air annealing. The one-element Ni1 oxide, two-element Ni1Co1 oxide, and three-element Ni1Co1Ag1 oxide two-dimensional catalysts prepared in the embodiments of the present invention can catalyze the reverse water-gas shift reaction with high selectivity and high efficiency. The synthesis method of the metal oxide two-dimensional catalyst provided by the present invention has the advantages of low preparation temperature, universality, simplicity, simple equipment, and environmental friendliness, and provides a new approach and new ideas for the field of catalytic reverse water-gas shift.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials and catalysts, and in particular to a low-temperature preparation method and application of a metal oxide two-dimensional catalyst. Background Art

[0002] In recent years, due to the massive consumption of fossil fuels and large-scale destruction of forests, the concentration of carbon dioxide in the atmosphere has risen rapidly over the past century, reaching an all-time high of 420.99ppm in 2022. Therefore, people have shown great interest and extensive exploration in the utilization of carbon dioxide and the catalytic conversion of carbon dioxide into valuable chemicals. In addition to reducing carbon dioxide emissions by means of energy conservation and emission reduction, researchers have also proposed strategies to capture and store carbon dioxide using porous materials. Among them, the reverse water gas shift reaction (RWGS) is considered to be a key intermediate step in the hydrogenation of carbon dioxide to produce high-value-added chemical products such as methane, methanol, and formic acid, and occupies an irreplaceable position in the conversion process of carbon dioxide. The reverse water gas shift reaction has many advantages such as abundant sources, low cost, and high output, but there are some problems with the catalysts used:

[0003] (1) Low catalyst activity and low carbon monoxide purity

[0004] The traditional catalysts used in the reverse water gas shift reaction include copper-based catalysts and ceria catalysts. However, due to the thermodynamic stability and kinetic inertness of carbon dioxide, it is difficult for traditional catalysts to efficiently convert it, and the catalysts have poor reduction resistance and stability. In addition, under the reaction conditions, byproducts such as methane will be generated, which will reduce the selectivity of carbon monoxide and result in low purity of carbon monoxide. In order to solve the problems of low catalyst activity and poor carbon monoxide selectivity, researchers currently use additive modification or special preparation methods to improve the activity of catalysts, but the final effect is not ideal.

[0005] (2) The catalyst preparation process is complicated and does not conform to the concept of green environmental protection.

[0006] The specific preparation process conditions of the catalyst have not been fully studied, and the results achieved are still only at the experimental small-scale production stage, which cannot meet the needs of industrialization. Traditional reverse water gas shift (RWGS) reaction catalysts are mostly oxide-supported catalysts, and the active components are precious metals and non-precious metal oxides. However, common precious metal catalysts such as Pt are difficult to industrialize due to their scarce resources and high prices; non-precious metals such as Ni, Co, Fe, and Cu also have catalytic activity in the RWGS reaction, but Cu-based catalysts and Fe-based catalysts are prone to sintering and agglomeration at high temperatures, resulting in low catalytic efficiency and poor thermal stability; Ni-based catalysts have good activity in the RWGS reaction, but they are prone to generate methane as a byproduct. Summary of the invention

[0007] The purpose of the present invention is to provide a low-temperature preparation method and application of a metal oxide two-dimensional catalyst to solve the problems of huge energy consumption, low catalyst efficiency, poor selectivity and inability to achieve industrialization in the existing reverse water-gas shift reaction.

[0008] The present invention is achieved as follows: a low-temperature preparation method for a metal oxide two-dimensional catalyst, specifically using water-soluble starch as a template, obtaining a precursor through freeze-drying technology, and then obtaining a two-dimensional catalyst through low-temperature slow annealing in air. The catalyst can be used for reverse water-gas shift reaction, with high catalytic efficiency and good selectivity.

[0009] Combination Figure 1 The present invention provides a universal low-temperature preparation method of metal oxide two-dimensional nanosheet catalysts, comprising the following steps:

[0010] 1) Dissolve a certain amount of water-soluble starch and metal salt in deionized water, stir evenly to form a mixed solution.

[0011] 2) Pour the mixed solution obtained in step 1) into liquid nitrogen and place it in a freeze dryer for 12 to 36 hours to obtain a catalyst precursor (the catalyst precursor becomes a solid).

[0012] 3) placing the catalyst precursor of step 2) into a muffle furnace, heating the temperature from room temperature to 300-500° C. in an air environment over 40-1500 min and maintaining the temperature for 3-8 h.

[0013] Furthermore, the metal salt in step 1) is nickel nitrate, cobalt nitrate and / or silver nitrate.

[0014] The present invention discloses a method for preparing a two-dimensional catalyst of monovalent Ni1 oxide, binary Ni1Co1 oxide and ternary Ni1Co1Ag1 oxide by utilizing the template method. The obtained two-dimensional catalyst has the characteristics of adjustable components and uniform element distribution, and the catalyst has a nano-sheet morphology structure.

[0015] The present invention further discloses that a two-dimensional catalyst of a monovalent Ni1 oxide, a binary Ni1Co1 oxide, or a ternary Ni1Co1Ag1 oxide is applied to a reverse water gas shift reaction. Specifically, a mixture of carbon dioxide and hydrogen is introduced into a reaction device at a CO2 / H2 molar ratio of 0.5 to 3.0, and the CO yield is tested by heating. The results show that the two-dimensional catalyst has good performance and selectivity for the reverse water gas shift reaction.

[0016] The subscripts of each element in the above-mentioned "binary Ni1Co1 oxide and ternary Ni1Co1Ag1 oxide two-dimensional catalysts" represent the molar ratio of the elements, indicating that the molar numbers of each element are the same. The subscript "1" of Ni in "monovalent Ni1 oxide" is for consistency with the labels of the other two substances and has no special meaning.

[0017] The present invention further discloses a Ni1 oxide catalyst prepared by a sol-gel method different from a starch template method as a comparative catalyst. It can be seen that the catalyst prepared by using starch as a template has the advantages of high activity and high selectivity.

[0018] The present invention has the following advantages:

[0019] 1) The temperature range of the method for preparing the two-dimensional catalyst of the present invention is 300-500°C, which greatly reduces the preparation temperature of the material.

[0020] 2) The equipment for preparing the two-dimensional catalyst of the present invention only requires a freeze dryer and a muffle furnace. Compared with other high-temperature smelting equipment for preparing high-entropy materials, it has the advantages of simple equipment and low cost.

[0021] 3) The present invention uses cheap starch as a template, and has the advantage of being able to prepare catalysts with high activity, high selectivity and high stability on a large scale.

[0022] 4) The preparation process of the present invention does not require water washing, and pure two-dimensional materials can be prepared, which is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a flow chart of the low-temperature preparation method of the metal oxide two-dimensional catalyst provided by the present invention.

[0024] Figure 2 This is a morphology characterization diagram of the monovalent Ni1 oxide obtained in Example 1.

[0025] Figure 3 This is a performance diagram of the CO yield of the thermal catalytic reverse water-gas shift reaction of the monovalent Ni1 oxide obtained in Example 1.

[0026] Figure 4 This is the CO selectivity diagram of the thermal catalytic reverse water gas shift reaction of the monovalent Ni1 oxide obtained in Example 1.

[0027] Figure 5 This is a performance diagram of the CO2 conversion rate of the thermal catalytic reverse water-gas shift reaction of the monovalent Ni1 oxide obtained in Example 1.

[0028] Figure 6 This is a performance diagram of the CO yield of the thermal catalytic reverse water-gas shift reaction of the monovalent Ni1 oxide obtained by the sol-gel method in Example 2.

[0029] Figure 7 This is a graph showing the CO selectivity of the thermally catalytic reverse water-gas shift reaction of the monovalent Ni1 oxide obtained by the sol-gel method in Example 2.

[0030] Figure 8 This is a morphology characterization diagram of the binary Ni1Co1 oxide obtained in Example 3.

[0031] Fig. 9 This is a performance diagram of the CO yield of the thermal catalytic reverse water gas shift reaction of the binary Ni1Co1 oxide obtained in Example 3.

[0032] Fig.10 This is the CO selectivity diagram of the thermal catalytic reverse water gas shift reaction of the binary Ni1Co1 oxide obtained in Example 3.

[0033] Fig.11 This is a performance diagram of the CO2 conversion rate of the thermal catalytic reverse water gas shift reaction of the binary Ni1Co1 oxide obtained in Example 3.

[0034] Fig.12 This is the structural characterization and morphological characterization diagram of the ternary Ni1Co1Ag1 oxide obtained in Example 4.

[0035] Fig.13 These are the high-resolution image, morphology image and element distribution image of the ternary Ni1Co1Ag1 oxide obtained in Example 4.

[0036] Fig.14 This is a performance diagram of the CO yield of the thermal catalytic reverse water gas shift reaction of the ternary Ni1Co1Ag1 oxide obtained in Example 4.

[0037] Fig.15 This is the CO selectivity diagram of the thermal catalytic reverse water gas shift reaction of the ternary Ni1Co1Ag1 oxide obtained in Example 4.

[0038] Fig.16 This is a performance diagram of the CO2 conversion rate of the thermal catalytic reverse water gas shift reaction of the ternary Ni1Co1Ag1 oxide obtained in Example 4. DETAILED DESCRIPTION

[0039] The specific implementation methods of the present invention are described in detail below with reference to implementation cases.

[0040] Example 1, preparation process of monovalent Ni1 oxide.

[0041] The synthesis steps of the monovalent Ni1 oxide two-dimensional nanosheet catalyst are as follows:

[0042] (1) Dissolve 1 g of water-soluble starch in 40 mL of deionized water and stir for 30 min.

[0043] (2) Add 100 mg of nickel nitrate to the water-soluble starch aqueous solution and stir to dissolve for 30 minutes.

[0044] (3) Freeze the above solution with liquid nitrogen and place it in a freeze dryer for freeze drying for 48 hours.

[0045] (4) Place the dried powder in a muffle furnace and heat it from room temperature to 425°C in an air environment over 1000 min and maintain it for 6 h. Allow the temperature to cool naturally and take out the sample for characterization. Figure 2 This is the morphology of Ni1 oxide. It can be seen from the figure that the catalyst presents a good nanosheet morphology.

[0046] Example 2, preparation process of monovalent Ni1 oxide by sol-gel method.

[0047] (1) Mix 5 g of citric acid and 1.339 g of nickel nitrate.

[0048] (2) Add 2.5 mL of nitric acid, 1 mL of ethylenediamine, and aqueous ammonia to the mixture until the pH is 6, and heat and stir until it becomes a gel.

[0049] (3) Place the above gel in an oven and dry at 80°C for 24 hours.

[0050] (4) The obtained gel was placed in a 400°C tubular furnace and calcined in argon for 3 h to obtain a precursor.

[0051] (5) The obtained precursor was placed in a muffle furnace, and the temperature was raised from room temperature to 450°C at a rate of 10°C / min in an air environment, and maintained for 6 hours. The temperature was naturally lowered, and the sample was taken out.

[0052] Example 3, preparation process of binary Ni1Co1 oxide.

[0053] The synthesis steps of binary Ni1Co1 oxide two-dimensional nanosheet catalyst are as follows:

[0054] (1) Dissolve 1 g of water-soluble starch in 40 mL of deionized water and stir for 30 min.

[0055] (2) Add 50 mg of nickel nitrate and 50 mg of cobalt nitrate to the water-soluble starch aqueous solution and stir to dissolve for 30 minutes.

[0056] (3) Freeze the above solution with liquid nitrogen and place it in a freeze dryer for freeze drying for 48 hours.

[0057] (4) Place the dried powder in a muffle furnace and heat it from room temperature to 425°C in an air environment over 1000 min and maintain it for 6 h. Allow the temperature to cool naturally and take out the sample for characterization. Figure 8This is the morphology of Ni1Co1 oxide. It can be seen from the figure that the catalyst presents a good nanosheet morphology.

[0058] Example 4, preparation process of ternary Ni1Co1Ag1 oxide.

[0059] The synthesis steps of the ternary Ni1Co1Ag1 oxide two-dimensional nanosheet catalyst are as follows:

[0060] (1) Dissolve 1 g of water-soluble starch in 40 mL of deionized water and stir for 30 min.

[0061] (2) Add 38.7 mg of nickel nitrate, 38.7 mg of cobalt nitrate, and 22.6 mg of silver nitrate to the water-soluble starch aqueous solution and stir to dissolve for 30 minutes.

[0062] (3) Freeze the above solution with liquid nitrogen and place it in a freeze dryer for 48 hours.

[0063] (4) Place the dried powder in a muffle furnace and heat it from room temperature to 425°C in an air environment for 1000 min and maintain it for 6 h. Allow the temperature to cool naturally and take out the sample for characterization. Fig.12 a is the X-ray diffraction pattern of Ni1Co1Ag1 oxide, showing the characteristic peak of Ag; Fig.12 b is the morphology of Ni1Co1Ag1 oxide. It can be seen from the figure that the catalyst presents a good nanosheet morphology. Fig.13 It is a high-resolution image, morphology image and element distribution map of Ni1Co1Ag1 oxide. The map shows that Co, Ni, and O elements are evenly dispersed in the two-dimensional Ni1Co1Ag1 oxide material, and the Ag element is slightly accumulated.

[0064] Example 5, application of monovalent Ni1 oxide catalyst.

[0065] 5 mg of the Ni1 oxide catalyst obtained in Example 1 was placed in a quartz tube and then placed in a tube furnace. Carbon dioxide and hydrogen were mixed in a ratio of 1:1 and injected into the reaction system to start the reaction. Each temperature point was maintained for 30 minutes and then the gas composition was detected by gas chromatography. The performance of the test is as follows: Figure 3 As shown in Figure 2, at 300 °C, the CO yield reached 93.1 mmol g - 1 h -1 ; Carbon monoxide selectivity is 96%, see Figure 4 The CO2 conversion rate is 0.99%, see Figure 5 .

[0066] Example 6, application of the monovalent Ni1 oxide catalyst obtained by the sol-gel method.

[0067] 5 mg of the Ni1 oxide catalyst obtained in Example 2 was placed in a quartz tube and then placed in a tube furnace. Carbon dioxide and hydrogen were mixed in a ratio of 1:1 and injected into the reaction system to start the reaction. Each temperature point was maintained for 30 minutes and then the gas composition was detected by gas chromatography. The performance of the test is as follows: Figure 6 As shown in Figure 2, only at 300 °C did the catalyst begin to be active, with a CO yield of 158.5 mmol g -1 h -1 ; Carbon monoxide selectivity is 65%, see Figure 7 , which is far lower than the monolithic Ni1 oxide catalyst prepared by starch template method.

[0068] Example 7, application of binary Ni1Co1 oxide catalyst.

[0069] 5 mg of the Ni1Co1 oxide catalyst obtained in Example 3 was placed in a quartz tube and then placed in a tube furnace. Carbon dioxide and hydrogen were mixed in a ratio of 1:1 and injected into the reaction system to start the reaction. Each temperature point was maintained for 30 minutes and then the gas composition was detected by gas chromatography. The performance of the test is as follows: Fig. 9 As shown in Figure 2, at 300 °C, the CO yield reached 312.62 mmol g -1 h -1 ; Carbon monoxide selectivity is 98.9%, see Fig.10 The CO2 conversion rate is 3.23%, see Fig.11 .

[0070] Example 8, application of ternary Ni1Co1Ag1 oxide catalyst.

[0071] 5 mg of the Ni1Co1Ag1 oxide catalyst obtained in Example 4 was placed in a quartz tube and then placed in a tube furnace. Carbon dioxide and hydrogen were mixed in a ratio of 1:1 and injected into the reaction system to start the reaction. Each temperature point was maintained for 30 minutes and then the gas composition was detected by gas chromatography. The performance of the test is as follows: Fig.14 As shown in Figure 2, at 300 °C, the CO yield reached 731.08 mmol g -1 h -1 ; Carbon monoxide selectivity is 97%, see Fig.15 The CO2 conversion rate is 7.7%, see Fig.16 .

Claims

1. Use of a metal oxide two-dimensional catalyst in catalyzing a reverse water gas shift reaction, characterized in that: The metal oxide two-dimensional catalyst is specifically a ternary NiCoAg oxide catalyst, wherein the molar ratio of Ni, Co and Ag is 1:1:1; the application is specifically: placing the ternary NiCoAg oxide catalyst in a quartz tube, and then placing it in a tubular furnace; mixing carbon dioxide and hydrogen in a ratio of 1:1 and injecting them into the reaction system for reaction; The preparation method of the ternary NiCoAg oxide catalyst is as follows: a. Dissolve water-soluble starch and metal salts of Ni, Co and Ag in deionized water, and stir evenly to form a mixed solution; b. pouring the mixed solution obtained in step a into liquid nitrogen, placing it in a freeze dryer for freeze drying, and obtaining a catalyst precursor; c. Put the catalyst precursor obtained in step b into a muffle furnace and anneal it in an air environment to obtain a ternary NiCoAg oxide catalyst.

2. The use according to claim 1, characterized in that: In step a, the mass of the metal salts of Ni, Co and Ag accounts for 5% to 15% of the mass of the water-soluble starch, and the mass of the water-soluble starch accounts for 1% to 10% of the mass of the deionized water.

3. The use according to claim 1, characterized in that: In step a, the metal salt is one or more of nitrate, acetate, chloride and sulfate.

4. The use according to claim 1, characterized in that: In step b, the freeze-drying time is 12 to 36 hours.

5. The use according to claim 1, characterized in that: In step c, the specific process of annealing is: heating from room temperature to 300-500°C in 40-1500 min and maintaining for 3-8 h.

Citation Information

Patent Citations

  • Composite metal oxide catalyst and application thereof

    CN111250077A

  • Preparation method and application of Co / Fe layered double-metal hydroxide nanosheet

    CN113493225A

  • Reverse water gas shift catalyst, preparation method and application thereof

    CN113908833A

  • Nanosheet catalyst for catalytic oxidation of VOC (Volatile Organic Compounds) as well as preparation and application methods of nanosheet catalyst

    CN114632516A

  • Low-temperature preparation method and application of high-entropy two-dimensional catalyst

    CN114950475A