A narrow bandgap bismuth sulfide nanoferroelectric semiconductor and its preparation and application

Bismuth sulfide nanoferroelectric semiconductors were synthesized by low-temperature hydrothermal reaction. The piezoelectric polarization of the surface free charges under ultrasonic irradiation was used to generate active oxygen free radicals, which solved the application problem of non-oxide nanoferroelectric materials in wastewater treatment and achieved efficient and low-cost wastewater treatment.

CN116078401BActive Publication Date: 2024-11-26TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211603709.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-26
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively utilize non-oxide nano-ferroelectric materials, especially narrow-bandgap ferroelectric semiconductors, in wastewater treatment. Furthermore, conventional wastewater treatment processes suffer from low efficiency, high energy consumption, and the generation of toxic sludge.

Method used

Narrow-bandgap bismuth sulfide nanoferroelectric semiconductors with different morphologies were synthesized by low-temperature hydrothermal reaction. The piezoelectric polarization intensity change of the surface free charge under ultrasonic irradiation was utilized to generate reactive oxygen free radicals, thereby achieving the oxidative decomposition of organic dyes in wastewater.

Benefits of technology

It achieves efficient and low-cost wastewater treatment, rapidly degrades dyes, is easy to promote, and is not limited by time and space, enriching our understanding of the properties of nano-ferroelectric materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116078401B_ABST
    Figure CN116078401B_ABST
Patent Text Reader

Abstract

The present invention relates to a narrow-bandgap bismuth sulfide nano-ferroelectric semiconductor and its preparation and application. The bismuth sulfide nano-ferroelectric semiconductor is synthesized by low-temperature hydrothermal reaction, wherein the bismuth sulfide nano-ferroelectric semiconductor includes two morphological structures, namely, irregular nanoparticle aggregates and nanorod aggregates. The narrow-bandgap bismuth sulfide nano-ferroelectric semiconductor prepared by the present invention has high efficiency in degrading organic dyes in wastewater under ultrasound. Compared with the prior art, the present invention prepares and synthesizes a bismuth sulfide nano-ferroelectric semiconductor rich in sulfur defects by a mild and inexpensive method. The semiconductor exhibits a high catalytic activity in degrading organic dyes in wastewater under ultrasound, enriches the research content of nano-ferroelectrics at the material level, expands the water treatment technology approach at the technical level, and the water purification process for degrading organic dyes in wastewater is easy to promote and apply on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferroelectric semiconductor preparation and water treatment, and in particular relates to a narrow-bandgap bismuth sulfide nano ferroelectric semiconductor and its preparation and application. Background Art

[0002] For a long time, the research on nano-ferroelectrics has mainly focused on perovskite-based composite oxides, while non-oxide ferroelectric materials, especially narrow-bandgap non-oxide ferroelectric semiconductors, have not received much attention due to their physical and chemical properties and application limitations. Therefore, breaking through the bottleneck of the preparation and application technology of non-oxide nano-ferroelectric semiconductors is an indispensable part of bridging the cognitive gap in nano-ferroelectric research.

[0003] Theoretical studies have shown that highly anisotropic ionic polarizabilities in sulfides can produce ferroelectric phase transitions. For example, Sb2S3 exhibits two ferroelectric phase transitions at 292 and 420 K, and this phase transition is similar to that of (Sb4S6) n The changes in the dipole moments of Sb and S atoms along the c-axis in the chain are closely related. n The anisotropy of the chain along the c-axis means that the macroscopic polarization of Sb2S3 is largely anisotropic. Although the synthesis of Bi2S3 nanostructures with different morphologies and their photoelectrochemical applications have been widely reported, there are very limited data on the ferroelectric behavior of nanoscale Bi2S3, including the application of its ferroelectric properties.

[0004] In view of the severe situation of water pollution and the difficulty in treating industrial wastewater discharged by industries such as printing and dyeing and papermaking, there is an urgent need to develop a new wastewater treatment technology that is low-cost, safe, reliable and easy to promote. At present, some conventional wastewater treatment processes, such as chemical precipitation, flotation and ion exchange, have disadvantages such as low removal efficiency, high energy consumption and the production of toxic sludge, which limits their widespread application. Various alternative treatment methods, such as adsorption using low-cost materials, membrane separation, electrocatalysis and photocatalysis technology, have expanded the scope of water purification applications to a certain extent, but there is still room for upgrading and improving efficiency. Summary of the invention

[0005] The purpose of the present invention is to provide a narrow-bandgap bismuth sulfide nano-ferroelectric semiconductor and its preparation and application.

[0006] The purpose of the present invention can be achieved by the following technical scheme: A method for preparing a narrow bandgap bismuth sulfide nano-ferroelectric semiconductor comprises the following steps:

[0007] Step (1): dissolving bismuth nitrate pentahydrate in ethylene glycol solvent and stirring with ultrasonic to obtain a transparent solution A;

[0008] Step (2): dissolving thiourea in a heated mixed solvent of polyethylene glycol and deionized water, and stirring to obtain a transparent solution B;

[0009] Step (3): slowly add the transparent solution A drop by drop into the transparent solution B, and continue to stir and mix to obtain a transparent yellow solution C;

[0010] Step (4): transferring solution C to a stainless steel polytetrafluoroethylene autoclave, reacting at a set reaction temperature for a period of time, and after the reaction is completed and the autoclave is cooled to room temperature, taking out the precipitate in the autoclave, washing it by centrifugation with ethanol and deionized water for 3 to 6 times respectively, and drying it to obtain a narrow band gap bismuth sulfide nano-ferroelectric semiconductor;

[0011] Among them, bismuth nitrate pentahydrate and thiourea are used as reactants, deionized water and ethylene glycol are used as reaction solvents, and polyethylene glycol is used as an additive. Nano ferroelectric semiconductor bismuth sulfide with different morphological structures is synthesized through low-temperature hydrothermal reaction.

[0012] Furthermore, the molar ratio of bismuth nitrate pentahydrate to thiourea is 1:(1-15).

[0013] Furthermore, the ultrasound in step (1) is to accelerate the dissolution rate of bismuth nitrate pentahydrate.

[0014] Furthermore, the concentration of bismuth nitrate pentahydrate in the transparent solution A in step (1) is 0.05 to 0.15 mol / L –1 .

[0015] Furthermore, the molecular weight of the polyethylene glycol described in step (2) is 6000, which has good adhesion and serves to increase the viscosity of the solvent; in the polyethylene glycol / deionized water solvent, the mass of the polyethylene glycol is 0.5 to 2.0 g, and the volume of the deionized water is 10 to 20 mL; and the washing with ethanol described in step (4) is to better remove the polyethylene glycol molecules remaining on the surface of the bismuth sulfide.

[0016] Furthermore, the concentration of thiourea in the transparent solution B in step (2) is 0.05 to 1.50 mol L –1 .

[0017] Furthermore, the reaction temperature in step (4) is 180-220° C., and the reaction time is 8-24 h.

[0018] Preferably, the reaction time in step (4) is 12 to 18 hours.

[0019] The second object of the present invention is to provide a narrow-bandgap bismuth sulfide nano-ferroelectric semiconductor prepared by the above method, wherein the narrow-bandgap bismuth sulfide nano-ferroelectric semiconductor has ferroelectric piezoelectric properties; the bismuth sulfide is composed of two morphological structures, namely, irregular nanoparticle aggregates (marked as Bi2S3) and nanorod aggregates (marked as v-Bi2S3), wherein the bismuth sulfide with different morphological structures is regulated by the molar ratio of bismuth nitrate pentahydrate and thiourea. When the molar ratio of bismuth nitrate pentahydrate and thiourea is 1:1, the synthesized bismuth sulfide is mainly irregular nanoparticle aggregates; when the molar ratio of bismuth nitrate pentahydrate and thiourea is 1:15, the synthesized bismuth sulfide is mainly nanorod aggregates.

[0020] The third object of the present invention is to provide an application of the above-mentioned narrow bandgap bismuth sulfide nanoferroelectric semiconductor, and to use the narrow bandgap bismuth sulfide nanoferroelectric semiconductor for water purification. Specifically, the narrow bandgap bismuth sulfide nanoferroelectric semiconductor is used to degrade organic dyes in wastewater, and the organic dyes include methyl orange, methyl blue and rhodamine B.

[0021] Furthermore, the specific application method of applying the narrow bandgap bismuth sulfide nanoferroelectric semiconductor to the degradation of organic dyes in wastewater is to disperse the bismuth sulfide in the wastewater containing the organic dyes and perform ultrasonic vibration to achieve the degradation of the organic dyes.

[0022] Furthermore, the power of the ultrasonic wave is 150-220W, and the vibration frequency is 20-50kHz.

[0023] The principle of the bismuth sulfide nano-ferroelectric semiconductor for degrading organic dyes in wastewater is that under the action of ultrasound, the free charges on the surface of bismuth sulfide are activated due to the periodic change of piezoelectric polarization intensity, and the "activated" charges undergo redox reactions with water molecules and dissolved oxygen to generate active oxygen free radicals, thereby achieving oxidative decomposition and removal of dye molecules.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] 1. The principle of the present invention to degrade organic dyes in wastewater by using bismuth sulfide nano-ferroelectric semiconductors prepared by low-temperature hydrothermal reaction is that under the action of ultrasound, the free charges on the surface of bismuth sulfide are activated due to the periodic change of piezoelectric polarization intensity, and the "activated" charges undergo redox reactions with water molecules and dissolved oxygen to generate active oxygen free radicals, thereby achieving oxidative decomposition and removal of dye molecules. Based on the piezoelectric theory (i.e., ferroelectric piezoelectric semiconductors can generate charges on their surfaces under mechanical stress) and the principles of mechanochemistry (using mechanical force to drive chemical reactions), the use of bismuth sulfide nano-ferroelectric semiconductors to remove organic dyes in wastewater not only enhances the understanding of the properties of non-oxide nano-ferroelectric materials, but also effectively improves water treatment methods, significantly increasing economic and social benefits;

[0026] 2. The bismuth sulfide nanoferroelectric semiconductor prepared by the present invention is rich in sulfur defects, exhibits ferroelectricity and piezoelectricity, and can respond to mechanical stress;

[0027] 3. The present invention proposes a water purification method using ultrasonic activation of bismuth sulfide to achieve dye degradation and removal. The catalytic degradation of dyes is fast and efficient, easy to promote, and the technology is not limited by time and space;

[0028] 4. The method for synthesizing bismuth sulfide of the present invention is low in cost and simple in process, and the prepared bismuth sulfide has high crystallinity and easy to control morphology. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Scanning electron micrographs of (a) random aggregates Bi2S3 and (b) nanorod aggregates v-Bi2S3 prepared at a molar ratio of bismuth nitrate pentahydrate to thiourea of ​​1:1 and 1:15, respectively;

[0030] Figure 2 Figure 2 shows the structural characteristics of bismuth sulfide with different morphological structures, (a, b) low-resolution transmission electron microscopy images of bismuth sulfide nanorods; (c) high-resolution transmission electron microscopy image of bismuth sulfide nanorods; (d) selected area electron diffraction image of bismuth sulfide nanorods; (e) high-angle annular dark field scanning transmission electron microscopy image of a single bismuth sulfide nanorod; EDS element distribution of Bi (f), S (g) and Bi / S (h) of a single bismuth sulfide nanorod; (i) XRD spectra of bismuth sulfide with different morphological structures; (j) EPR spectra of bismuth sulfide with different morphological structures; (k) piezoelectric response amplitude-potential and phase-potential curves of bismuth sulfide nanorods;

[0031] Figure 3 Force scanning microscope amplitude (left) and phase (right) images of the piezoelectric response of bismuth sulfide nanorods;

[0032] Figure 4 Diffuse reflectance UV-visible absorption spectra (a) and XPS valence band spectra (b) of bismuth sulfide with different morphologies and structures;

[0033] Figure 5 N2 adsorption / desorption isotherms of bismuth sulfide with different morphologies and pore size distributions determined by the BJH method (inset);

[0034] Figure 6 The EPR spectra of oxygen free radicals generated by bismuth sulfide with different morphologies and structures under ultrasound;

[0035] Figure 7 This is a comparison chart of the degradation efficiency and reaction rate of bismuth sulfide with different morphologies and structures on dye wastewater under ultrasound;

[0036] Figure 8 This is the degradation efficiency curve of bismuth sulfide with different morphologies and structures on methyl orange dye wastewater under natural light. DETAILED DESCRIPTION

[0037] The present invention will be described in detail below with reference to the accompanying drawings and embodiments. It should be noted that, for those skilled in the art, several changes and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

[0038] The reagents used in the following examples are all commercially available reagents. The equipment used in the following examples are all commercially available equipment.

[0039] Example 1

[0040] 0.49 g of bismuth nitrate pentahydrate was weighed and dissolved in 15 mL of ethylene glycol under ultrasonic action to form a clear transparent solution A; 0.07 g of thiourea was weighed and dissolved in 15 mL of deionized water (containing 1.0 g of polyethylene glycol) under stirring to form a transparent solution B; the transparent solution A was added dropwise to the transparent solution B, mixed evenly, and continuously stirred to form a transparent yellow solution C; the yellow solution C was transferred to a high-pressure reactor, kept at 200° C. for reaction for 12 hours, and the reactor was cooled to room temperature, the precipitate in the reactor was taken out and centrifuged and washed 3 to 5 times with ethanol and deionized water, and then dried at 60° C. to obtain bismuth sulfide with irregular nanoparticle aggregates.

[0041] Example 2

[0042] 0.49 g of bismuth nitrate pentahydrate was weighed and dissolved in 15 mL of ethylene glycol under ultrasonic action to form a clear transparent solution A; 1.14 g of thiourea was weighed and dissolved in 15 mL of deionized water (containing 1.0 g of polyethylene glycol) under stirring to form a transparent solution B; the transparent solution A was added dropwise to the transparent solution B, mixed evenly, and stirred continuously to form a transparent yellow solution C; the yellow solution C was transferred to a high-pressure reactor, kept at 200° C. for reaction for 12 hours, and after the reactor was cooled to room temperature, the precipitate in the reactor was taken out and washed by centrifugation with ethanol and deionized water for 3 to 5 times, and dried at 60° C. to obtain bismuth sulfide nanorod aggregates.

[0043] Example 3

[0044] 0.37 g of bismuth nitrate pentahydrate was weighed and dissolved in 15 mL of ethylene glycol under ultrasonic action to form a clear transparent solution A; 0.04 g of thiourea was weighed and dissolved in 10 mL of deionized water (containing 0.5 g of polyethylene glycol) under stirring to form a transparent solution B; the transparent solution A was added dropwise to the transparent solution B, mixed evenly, and continuously stirred to form a transparent yellow solution C; the yellow solution C was transferred to a high-pressure reactor, kept warm at 180° C. for reaction for 8 hours, and the reactor was cooled to room temperature, the precipitate in the reactor was taken out and washed by centrifugation with ethanol and deionized water for 3 to 5 times, and dried at 60° C. to obtain bismuth sulfide nanoparticles.

[0045] Example 4

[0046] 1.09 g of bismuth nitrate pentahydrate was weighed and dissolved in 15 mL of ethylene glycol under ultrasonic action to form a clear transparent solution A; 2.28 g of thiourea was weighed and dissolved in 20 mL of deionized water (containing 2.0 g of polyethylene glycol) under stirring to form a transparent solution B; the transparent solution A was added dropwise to the transparent solution B, mixed evenly, and continuously stirred to form a transparent yellow solution C; the yellow solution C was transferred to a high-pressure reactor, kept at 220° C. for reaction for 24 hours, and the reactor was cooled to room temperature, the precipitate in the reactor was taken out and washed by centrifugation with ethanol and deionized water for 3 to 5 times, and dried at 60° C. to obtain bismuth sulfide nanorods.

[0047] The characterization results of bismuth sulfide with different morphologies and structures prepared in Examples 1 and 2 of the present invention are as follows:

[0048] Figure 1 The bismuth sulfide with different morphological structures is shown. Among them, under the equimolar ratio of bismuth nitrate pentahydrate and thiourea, the prepared bismuth sulfide is mainly composed of irregular nanoparticles, such as Figure 1 As shown in a; under the reaction conditions where the molar ratio of bismuth nitrate pentahydrate to thiourea is 1:15, the synthesized bismuth sulfide is mainly composed of nanorods, such as Figure 1 As shown in b.

[0049] Figure 2 The structural characteristics of bismuth sulfide with different morphological structures are shown in Figure 2. Figure 2 ac are low-resolution and high-resolution transmission electron microscopy images of bismuth sulfide nanorods. It can be seen that the length of the bismuth sulfide nanorods is 100-350nm, and the high-resolution lattice fringe spacing belongs to the (130) crystal plane; Figure 2 The selected area electron diffraction (d) shows that the prepared bismuth sulfide nanorods are single crystals. Figure 2 eh, it can be seen that Bi and S elements are evenly distributed on the surface of single-crystal bismuth sulfide nanorods; Figure 2 i shows that the synthesized bismuth sulfide belongs to the orthorhombic system and the space group is Pbnm(62); Figure 2j shows that the sulfur vacancy defect content of bismuth sulfide nanorods is higher than that of random aggregated bismuth sulfide, because the electron spin resonance spectrum (EPR) intensity of bismuth sulfide nanorods near the g value is higher. This means that the carrier concentration of bismuth sulfide nanorods is higher, which is conducive to inducing more surface free activated charges under ultrasound, thereby improving the redox catalytic efficiency. Through piezoelectric response force scanning microscopy, under ±10V AC voltage scanning, bismuth sulfide nanorods ( Figure 2 k) A symmetrical piezoelectric response amplitude-potential curve is presented, indicating that bismuth sulfide nanorods have piezoelectricity. The phase angle flips 180° under ±10V AC voltage scanning, indicating that bismuth sulfide nanorods have ferroelectricity.

[0050] Figure 3 Figure 1 shows the amplitude (left) and phase (right) of the piezoelectric response force scanning microscope of bismuth sulfide nanorods. 2 In this area, the potential amplitude change (ΔV=8.5mV) and phase reversal (Δθ=180deg.) of bismuth sulfide nanorods under ±10V AC voltage scanning can be observed, which indicates that bismuth sulfide nanorods produce inverse piezoelectric effect and spontaneous polarization moment under the action of AC voltage, proving that bismuth sulfide nanorods have piezoelectric response properties and ferroelectricity.

[0051] Figure 4 The diffuse reflectance UV-visible absorption spectra (a) and XPS valence band spectra (b) of bismuth sulfide with different morphologies and structures, where F(R∞) is the Kubelka–Munk function. Figure 3 a It can be seen that the light response performance of bismuth sulfide nanorods is higher than that of random aggregates of bismuth sulfide, and their band gaps are all less than 1.00 eV, and they have strong absorption properties for visible light. Figure 3 b It is known that the valence band and conduction band positions of bismuth sulfide with different morphological structures do not meet the thermodynamic conditions for the generation of oxygen free radicals, which further confirms that the water purification effect based on bismuth sulfide is attributed to the surface activated free charges generated by bismuth sulfide induced by ultrasonic vibration.

[0052] Figure 5 The N2 adsorption / desorption isotherms of bismuth sulfide with different morphologies and the pore size distribution determined by the BJH method (inset). It can be seen from the figure that the pore structure of the synthesized bismuth sulfide is composed of micropores and macropores. The specific surface areas of the random aggregates and nanorod aggregates are 16.65 and 14.10 m 2 / g.

[0053] Figure 6The following are the EPR spectra of oxygen free radicals generated by bismuth sulfide with different morphologies under ultrasound. The reaction conditions are consistent with those for dye degradation. As can be seen from the figure, the activity of nanorod bismuth sulfide in generating oxygen free radicals is higher than that of random aggregate bismuth sulfide, which is why nanorod bismuth sulfide has a higher catalytic performance in degrading organic dyes under ultrasound activation.

[0054] The specific steps of using the bismuth sulfide nano-ferroelectric semiconductor of the present invention to degrade organic dyes in wastewater are as follows:

[0055] Weigh bismuth sulfide and disperse it in an organic dye wastewater solution with a concentration of 10ppm, let it stand for 30s, and the concentration of bismuth sulfide in the wastewater solution is 0.5ppb; float the container containing the bismuth sulfide aqueous solution in an ultrasonic instrument with a rated water level, and the water level and temperature of the ultrasonic instrument are controlled by long-flowing water; ultrasonicate for a certain time, remove the supernatant, further centrifuge to remove bismuth sulfide, and use a spectrophotometer to detect the concentration of the dye in the centrifuge. The above reaction is carried out under dark room conditions to eliminate the interference of natural light on the reaction efficiency.

[0056] Three groups of blank control groups were set up: the first group was an equal volume of wastewater solution without bismuth sulfide and ultrasonic treatment to exclude the effect of bismuth sulfide in the purified water; the second group was an equal volume of wastewater solution containing bismuth sulfide, but no ultrasonic treatment was applied to exclude the effect of ultrasound in the purified water; the third group was an equal volume of wastewater solution with bismuth sulfide added and placed under natural light conditions, but no ultrasonic treatment was applied to explore the effect of natural light on the reaction system.

[0057] Figure 7 The figure shows the degradation efficiency and reaction rate comparison of bismuth sulfide with different morphologies and structures on dye wastewater under ultrasound. It can be seen from the figure that the degradation activity and corresponding reaction rate constant of nanorod bismuth sulfide on rhodamine B, methyl orange and methyl blue dyes are significantly higher than those of random aggregate bismuth sulfide, which shows that the axial structure of nanorods and high concentration of sulfur defects play a key role in improving the catalytic efficiency of bismuth sulfide.

[0058] Figure 8 The degradation efficiency curve of bismuth sulfide with different morphologies and structures for wastewater containing methyl orange dye under natural light. Obviously, under natural light irradiation, the dye concentration did not change within 6 minutes, which shows that bismuth sulfide does not have catalytic activity for degrading methyl orange dye under natural light, highlighting the advantage of bismuth sulfide's high catalytic activity under ultrasound.

[0059] The present invention prepares and synthesizes sulfur-defect-rich bismuth sulfide nanoferroelectric semiconductors by a mild and inexpensive method. The semiconductors show high catalytic activity in degrading organic dyes in wastewater under ultrasound, enriches the research content of nanoferroelectrics at the material level, expands the water treatment technology approach at the technical level, and the water purification process is easy to promote and apply on a large scale.

[0060] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An application of a narrow bandgap bismuth sulfide nanoferroelectric semiconductor, characterized in that: The method for preparing the narrow bandgap bismuth sulfide nano-ferroelectric semiconductor comprises the following steps: Step (1): dissolving bismuth nitrate pentahydrate in ethylene glycol solvent and stirring to obtain a transparent solution A; Step (2): dissolving thiourea in a polyethylene glycol / deionized water solvent and stirring to obtain a transparent solution B, wherein the polyethylene glycol in the polyethylene glycol / deionized water solvent has a mass of 0.5-2.0 g and a volume of deionized water of 10-20 mL; Step (3): adding transparent solution A dropwise into transparent solution B, and continuously stirring to obtain solution C; Step (4): transferring solution C to a high-pressure reactor for reaction. After the reaction is completed, taking out the precipitate in the reactor, washing it, and drying it to obtain a narrow-bandgap bismuth sulfide nano-ferroelectric semiconductor. The reaction temperature in step (4) is 180-220°C, and the reaction time is 8-24 h; The molar ratio of the bismuth nitrate pentahydrate to thiourea is 1:(1-15); The narrow bandgap bismuth sulfide nano-ferroelectric semiconductor is rich in sulfur defects and has ferroelectric piezoelectric properties; the bismuth sulfide is composed of two morphological structures: irregular nanoparticle aggregates and nanorod aggregates; The narrow bandgap bismuth sulfide nano-ferroelectric semiconductor is applied to degrade organic dyes in wastewater. The specific application method is to disperse bismuth sulfide in wastewater containing organic dyes and use ultrasonic vibration to achieve degradation of the organic dyes.

2. The use of a narrow bandgap bismuth sulfide nanoferroelectric semiconductor according to claim 1, characterized in that: The concentration of bismuth nitrate pentahydrate in the transparent solution A described in step (1) is 0.05-0.15 mol L –1 .

3. The use of a narrow bandgap bismuth sulfide nano-ferroelectric semiconductor according to claim 1, characterized in that: The molecular weight of the polyethylene glycol described in step (2) is 6000.

4. The use of a narrow bandgap bismuth sulfide nano-ferroelectric semiconductor according to claim 1, characterized in that: The concentration of thiourea in the transparent solution B in step (2) is 0.05-1.50 mol L –1 .

5. The use of a narrow bandgap bismuth sulfide nano-ferroelectric semiconductor according to claim 1, characterized in that: The power of the ultrasonic wave is 150-220 W, and the vibration frequency is 20-50 kHz.