Method for recovering waste liquid containing cobalt and rare earth
By replacing copper removal, oxidation precipitation and chemical precipitation in cobalt-containing rare earth waste liquid, the problem of incomplete recycling is solved, and efficient recycling and low pollution are achieved.
Patent Information
- Application Number
- CN202310091139.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-02-09
AI Technical Summary
The waste liquid containing cobalt is not completely recovered in the prior art, resulting in low economic benefits and high environmental pollution.
Copper is removed by adding a replacer to the cobalt-containing rare earth waste liquid, and then oxidative precipitation and chemical precipitation are carried out in the copper removal liquid, copper, rare earth, nickel, and cobalt metal are recovered in steps, and salts in the wastewater are recovered by evaporation and crystallization. substance.
It has achieved efficient recycling of copper, rare earths, nickel and cobalt, reduced recycling costs and processes, improved economic benefits, and basically achieved zero emissions and low environmental pollution.
Smart Images

Figure BDA0004070400110000061 
Figure BDA0004070400110000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of industrial wastewater treatment, and in particular to a method for recovering cobalt-containing rare earth waste liquid. Background Art
[0002] Industrial production in the rare earth industry generates cobalt-containing wastewater, which contains small amounts of copper, nickel, and rare earth metals, offering considerable recycling value. The existing treatment method involves direct precipitation with lime milk, adjusting the pH to alkaline to precipitate these metals into the slag. While this method is simple and easy to implement, the resulting slag contains a large amount of gypsum, and copper, cobalt, nickel, and rare earth elements are mixed together, making it of low value. Furthermore, the slag is considered hazardous waste and cannot be directly stored, resulting in significant environmental pollution. Summary of the Invention
[0003] The main purpose of the present invention is to provide a method for recovering cobalt-containing rare earth waste liquid, so as to solve the problem in the prior art that incomplete recovery of cobalt-containing rare earth waste liquid leads to low economic benefits and serious environmental pollution.
[0004] In order to achieve the above-mentioned object, according to one aspect of the present invention, a method for recovering cobalt-containing rare earth waste liquid is provided, wherein the metal elements of the cobalt-containing rare earth waste liquid include copper, nickel, cobalt and rare earth elements, and the anions of the cobalt-containing rare earth waste liquid include chloride ions. The recovery method comprises the following steps: step S1, adding a displacing agent to the cobalt-containing rare earth waste liquid to displace and remove copper, thereby obtaining sponge copper and a copper-removed liquid; step S2, sequentially adding a first oxidant and lime milk to the copper-removed liquid, adjusting the pH to 4.0-5.0 to remove the displacing agent, thereby obtaining a displacing agent-rare earth mixed solution. slag and a liquid after removing the displacing agent; step S3, sequentially adding a second oxidant and lime milk to the liquid after removing the displacing agent, adjusting the pH to 4.0-5.0 to precipitate cobalt to obtain a high-valent oxide of cobalt and a liquid after cobalt precipitation; step S4, adding lime milk to the liquid after cobalt precipitation to precipitate nickel, adjusting the pH to 7.5-8.5 to obtain nickel hydroxide and a liquid after nickel precipitation; step S5, evaporating and crystallizing the liquid after nickel precipitation to obtain a crystalline salt, which includes calcium chloride; wherein the displacing agent is iron powder and / or aluminum powder; and the oxidizing property of the first oxidant is lower than that of the second oxidant.
[0005] Furthermore, in step S1, the dosage coefficient of the displacing agent is 1.0 to 5.0; preferably, the displacement temperature in step S1 is 30 to 80°C, and the displacement time is 5 to 120 minutes.
[0006] Furthermore, in step S2, the first oxidant is one or more of hydrogen peroxide, oxygen and air.
[0007] Furthermore, in step S2, the dosage coefficient of the first oxidant is 1.0 to 2.0; preferably, the reaction temperature of step S2 is 30 to 80°C, and the reaction time is 0.5 to 5 hours.
[0008] Furthermore, in step S3, the second oxidant is one or more of persulfate, chlorate, sulfur dioxide and ozone; preferably, the persulfate is one or more of potassium persulfate, sodium persulfate and calcium persulfate; preferably, the chlorate is one or more of potassium chlorate, sodium chlorate and calcium chlorate; preferably, the volume concentration of sulfur dioxide and / or ozone is 0.1 to 2 vol%.
[0009] Furthermore, in step S3, the dosage coefficient of the second oxidant is 1.0 to 2.0; preferably, the reaction temperature of step S3 is 30 to 80° C., and the reaction time is 0.5 to 5 h; more preferably, the reaction temperature of step S4 is 30 to 80° C., and the reaction time is 0.5 to 5 h.
[0010] Furthermore, in step S5, the temperature of the evaporation crystallization is 70-100° C., and the time is 0.5-3 h.
[0011] Furthermore, measured by mass concentration, the cations in the cobalt-containing rare earth waste liquid include 8 to 15 g / L of cobalt ions, 0.5 to 3 g / L of nickel ions, 1 to 5 g / L of copper ions, and 0.01 to 1 g / L of rare earth element ions, and the rare earth element ions include one or more of Nd, Sm, Tb and Dy.
[0012] Furthermore, the pH of the cobalt-containing rare earth waste liquid is 0.8 to 1.2.
[0013] Furthermore, the cobalt recovery rate in the cobalt-containing rare earth waste liquid is ≥99%, the nickel recovery rate is ≥98%, and the copper recovery rate is ≥92%.
[0014] The technical solution of the present invention is used to recover cobalt-containing wastewater containing small amounts of copper, nickel, and rare earths generated during the rare earth production process. First, copper is removed by displacement, followed by iron and aluminum removal and rare earth enrichment. Cobalt is then oxidized and precipitated, followed by nickel chemical precipitation. Finally, salts in the wastewater are recovered. Through staged precipitation, the copper, rare earth, nickel, and cobalt metals are recovered step by step. The products are sold and processed separately. This method has low recovery costs, a short recovery process, and a simple and easy-to-operate recovery method. Various metals are recovered more thoroughly, significantly improving economic benefits. Furthermore, the final wastewater of this method is a salt primarily composed of calcium chloride, which is recovered by evaporation and crystallization. The evaporated condensate can be reused in the rare earth production system, essentially achieving zero emissions and minimizing environmental pollution. DETAILED DESCRIPTION
[0015] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the embodiments.
[0016] Explanation of terms:
[0017] Dosage coefficient: stoichiometric ratio, that is, the ratio of the balanced values according to the reaction equation. In this case, the dosage coefficient is 1. When the dosage coefficient is 1.1, it means that the substance is 10% in excess.
[0018] As described in the background technology of the present invention, there are problems in the prior art of incomplete recovery of cobalt-containing rare earth waste liquid and low economic benefits. In order to solve the above problems, in a typical embodiment of the present invention, a method for recovering cobalt-containing rare earth waste liquid is provided, wherein the metal elements of the cobalt-containing rare earth waste liquid include copper, nickel, cobalt and rare earth elements, and the anions of the cobalt-containing rare earth waste liquid include chloride ions. The recovery method comprises the following steps: step S1, adding a displacer to the cobalt-containing rare earth waste liquid to displace and remove copper, thereby obtaining sponge copper and a copper-removed liquid; step S2, sequentially adding a first oxidant and lime milk to the copper-removed liquid, adjusting the pH to 4.0-5.0 to remove the displacer, and obtaining a displacer-rare earth liquid. Mixing the slag and the liquid after the displacing agent is removed; step S3, sequentially adding a second oxidant and lime milk to the liquid after the displacing agent is removed, adjusting the pH to 4.0-5.0 to precipitate cobalt, thereby obtaining a high-valent oxide of cobalt and a liquid after the cobalt precipitation; step S4, adding lime milk to the liquid after the cobalt precipitation to precipitate nickel, adjusting the pH to 7.5-8.5, thereby obtaining nickel hydroxide and a liquid after the nickel precipitation; step S5, evaporating and crystallizing the liquid after the nickel precipitation to obtain a crystalline salt, wherein the crystalline salt includes calcium chloride; wherein the displacing agent is iron powder and / or aluminum powder; and the oxidizing property of the first oxidant is lower than that of the second oxidant.
[0019] In the process of recovering cobalt-containing waste liquid with a small amount of copper, nickel and rare earth generated in the rare earth production process, the present invention first adds a displacing agent to the cobalt-containing rare earth waste liquid to displace and remove copper, wherein the displacing agent is iron powder and / or aluminum powder, and first displaces the copper element to obtain sponge copper and a copper-removed liquid; then, a first oxidant and lime milk are sequentially added to the copper-removed liquid, and the pH is adjusted to 4.0-5.0 to remove the displacing agent, wherein the first oxidant has a relatively weak oxidizing property and can only oxidize and precipitate iron, aluminum and rare earth to obtain a displacing agent-rare earth mixed slag and a displacing agent-removed liquid; then, a second oxidant and lime milk are sequentially added to the displacing agent-removed liquid, and the pH is adjusted to 4.0-5.0. The method comprises the following steps: cobalt precipitation is carried out at a pH of 4.0 to 5.0, wherein the second oxidant has a strong oxidizing property and can oxidize and precipitate the cobalt, and nickel will not be precipitated under the above-mentioned slightly acidic pH conditions, thereby obtaining a relatively pure high-valent oxide of cobalt and a cobalt precipitation liquid; lime milk is then added to the cobalt precipitation liquid to precipitate nickel, and the pH is adjusted to 7.5 to 8.5. Under higher pH conditions, nickel is directly precipitated to obtain nickel hydroxide and a nickel precipitation liquid, and copper, rare earth, nickel and cobalt metals are recovered step by step through a staged precipitation method. The products are sold and processed separately, with low recovery cost, short recovery process, simple and easy operation, more thorough recovery of various metals, and greatly improved economic benefits. Finally, the final wastewater nickel precipitation liquid of the method is evaporated and crystallized to obtain a crystalline salt mainly composed of calcium chloride. The evaporated condensed water can also be returned to the rare earth production system for use, basically achieving zero emission and low environmental pollution.
[0020] Typically, but not limiting, the pH in step S2 is 4.0, 4.2, 4.4, 4.5, 4.6, 4.8, 5.0; the pH in step S3 is 4.0, 4.2, 4.4, 4.5, 4.6, 4.8, 5.0; and the pH in step S4 is 7.5, 7.7, 7.9, 8.0, 8.1, 8.3, 8.5.
[0021] In a preferred embodiment, in step S1, the dosage coefficient of the replacement agent is 1.0 to 5.0, which can more fully replace the copper in the wastewater, further improve the copper recovery rate, and at the same time minimize the amount of reagent used, thereby further reducing the recovery cost; in order to increase the replacement reaction rate and further shorten the recovery process, preferably, the replacement temperature in step S1 is 30 to 80° C., and the replacement time is 5 to 120 min.
[0022] The oxidizing agent used to oxidize iron or aluminum, and rare earth elements should not be too strong, otherwise it will easily oxidize cobalt, resulting in difficulty in separating the precipitate after adding lime milk. Therefore, in a preferred embodiment, in step S2, the first oxidant is one or more of hydrogen peroxide, oxygen and air. The oxidizing properties of the above oxidants can oxidize iron or aluminum, and rare earth elements and then precipitate them into the slag without oxidizing cobalt and affecting the subsequent recovery of cobalt. The recovery of various elements is more thorough, and the economic benefits are further improved.
[0023] In order to achieve sufficient oxidation while saving costs, in a preferred embodiment, in step S2, the dosage coefficient of the first oxidant is 1.0 to 2.0; to further increase the oxidation reaction rate of step S2, preferably, the reaction temperature of step S2 is 30 to 80°C, and the reaction time is 0.5 to 5h.
[0024] The first oxidant has a relatively weak oxidizing property and cannot completely oxidize the cobalt in the wastewater. Therefore, in a preferred embodiment, in step S3, the second oxidant is one or more of persulfate, chlorate, sulfur dioxide, and ozone. Preferably, the persulfate is one or more of potassium persulfate, sodium persulfate, and calcium persulfate. Preferably, the chlorate is one or more of potassium chlorate, sodium chlorate, and calcium chlorate. Preferably, the volume concentration of sulfur dioxide and / or ozone is 0.1-2 vol%, where the volume concentration refers to the concentration of the mixed gas of sulfur dioxide and / or ozone and air or oxygen relative to oxygen. Persulfate is relatively stable and has strong oxidizing properties, and has the advantages of low toxicity, low price, and easy operation. Chlorate contains trigonal pyramidal chlorate ions, in which the oxidation state of the chlorine atom is +5, and therefore has strong oxidizing properties. The above oxidants can fully oxidize the cobalt in the wastewater, allowing for more complete cobalt metal recovery, thereby further improving the economic benefits of rare earth wastewater recovery according to the present invention.
[0025] In a preferred embodiment, in step S3, the dosage coefficient of the second oxidant is 1.0 to 2.0. The above dosage of the second oxidant can achieve a good cobalt oxidation effect without causing side reactions of other components in the wastewater solution to affect the metal recovery effect due to excessive addition of a strong oxidant; preferably, the reaction temperature of step S3 is 30 to 80°C, and the reaction time is 0.5 to 5h; more preferably, the reaction temperature of step S4 is 30 to 80°C, and the reaction time is 0.5 to 5h. Under the above temperature and time conditions, the precipitation rate of cobalt and nickel in the wastewater is faster, which is conducive to further shortening the recovery process and reducing the recovery cost.
[0026] The evaporation crystallization can use the commonly used process parameters in the art. In a preferred embodiment, in step S5, the evaporation crystallization temperature is 70-100° C. and the time is 0.5-3 h, which is more suitable for the treatment of saline wastewater of the present invention.
[0027] In order to make the recovery method of the present invention more in line with production practice, in a preferred embodiment, the cations in the cobalt-containing rare earth waste liquid include cobalt ions 8 to 15 g / L, nickel ions 0.5 to 3 g / L, copper ions 1 to 5 g / L, rare earth element ions 0.01 to 1 g / L, rare earth element ions include one or more of Nd, Sm, Tb and Dy, and anions include chloride ions. The above-mentioned cobalt-containing rare earth waste liquid is more suitable for the recovery method of the present invention, and the metal elements contained therein with a specific mass concentration can be more thoroughly recovered, with higher economic benefits.
[0028] In a preferred embodiment, the pH of the cobalt-containing rare earth wastewater is 0.8-1.2. Under the above pH conditions, the presence of various metal elements in the cobalt-containing rare earth wastewater is more stable, which is more convenient for subsequent recovery operations using the method of the present invention.
[0029] The recovery method of the present invention can achieve good recovery effects. In a preferred embodiment, the cobalt recovery rate in the cobalt-containing rare earth waste liquid is ≥99%, the nickel recovery rate is ≥98%, and the copper recovery rate is ≥92%.
[0030] The present application is further described in detail below with reference to specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application.
[0031] Example 1
[0032] The composition of the cobalt-containing rare earth waste liquid (measured by mass concentration) is: cobalt 8g / L, nickel 0.8g / L, copper 5g / L, rare earth elements 0.2g / L, and pH 1.
[0033] Step S1: adding iron powder to the cobalt-containing rare earth waste liquid to replace copper, the iron powder dosage coefficient is 1.8, the replacement temperature is 80° C., the replacement time is 10 min, and filtering is performed to finally obtain sponge copper and a copper-removed liquid.
[0034] In step S2, the copper-removed liquid is subjected to iron removal, and hydrogen peroxide is added for weak oxidation, with a hydrogen peroxide dosage coefficient of 1.5, an iron removal temperature of 80° C., and a reaction time of 3 hours. Then, lime milk is used as a neutralizer, and the end point pH of the solution system is controlled at 4.6. The solution is filtered to obtain rare earth-enriched iron hydroxide slag, which is returned to the rare earth production system for recovery, and the iron-removed liquid is obtained at the same time.
[0035] Step S3, precipitating cobalt from the deironing liquid, controlling the pH of the deironing liquid at 4.6, adding sodium persulfate, and adding lime milk to stabilize the pH, oxidizing and precipitating the cobalt in the solution, the sodium persulfate dosage coefficient is 1.5, the cobalt precipitation temperature is 80°C, the reaction time is 2 hours, filtering, and obtaining a high-valent oxide of cobalt and the cobalt precipitation liquid.
[0036] Step S4, precipitating nickel from the cobalt precipitation solution, using lime milk to precipitate nickel, controlling the end point pH of the solution system to 8.0, the nickel precipitation temperature to 80° C., the reaction time to 2 h, and filtering to obtain nickel hydroxide and the nickel precipitation solution.
[0037] Step S5, evaporating and crystallizing the nickel-precipitated solution at a crystallization temperature of 90° C. for 2 hours, and finally obtaining a salt product mainly composed of calcium chloride.
[0038] Example 2
[0039] The difference between Example 2 and Example 1 is that the composition of the cobalt-containing rare earth waste liquid (measured by mass concentration) is: 8 g / L cobalt, 3 g / L nickel, 5 g / L copper, 1 g / L rare earth element, and pH is 0.8.
[0040] Example 3
[0041] The difference between Example 3 and Example 1 is that the composition of the cobalt-containing rare earth waste liquid (measured by mass concentration) is: 15 g / L cobalt, 0.5 g / L nickel, 1 g / L copper, 1 g / L rare earth elements, and pH is 1.2.
[0042] Example 4
[0043] The difference between Example 4 and Example 1 is that in step S1, the displacing agent is aluminum powder, the dosage coefficient is 1.0, the displacement temperature is 80° C., and the displacement time is 5 min.
[0044] Example 5
[0045] The difference between Example 5 and Example 1 is that in step S1, the displacing agent is aluminum powder, the dosage coefficient is 5.0, the displacement temperature is 30° C., and the displacement time is 120 min.
[0046] Example 6
[0047] The difference between Example 6 and Example 1 is that in step S2, oxygen is introduced for weak oxidation, the oxygen usage coefficient is 1.0, the iron removal temperature is 80°C, the reaction time is 0.5h, and then lime milk is used as a neutralizer to control the end point pH of the solution system at 4.0; in step S3, the pH of the liquid after iron removal is controlled at 4.0.
[0048] Example 7
[0049] The difference between Example 7 and Example 1 is that in step S2, air is introduced for weak oxidation, the oxygen usage coefficient is 2.0, the iron removal temperature is 30°C, the reaction time is 5 hours, and then lime milk is used as a neutralizer to control the endpoint pH of the solution system at 5.0. In step S3, the pH of the liquid after iron removal is controlled at 5.0.
[0050] Example 8
[0051] The difference between Example 8 and Example 1 is that in step S3, the pH of the liquid after iron removal is controlled at 4.0, potassium chlorate is added, and lime milk is added to stabilize the pH, the sodium persulfate dosage coefficient is 1.0, the cobalt precipitation temperature is 30°C, and the reaction time is 5 hours.
[0052] Example 9
[0053] The difference between Example 9 and Example 1 is that in step S3, the pH of the liquid after iron removal is controlled at 5.0, sulfur dioxide (volume concentration is 0.1 vol%) is added, and lime milk is added to stabilize the pH, the sodium persulfate dosage coefficient is 2.0, the cobalt precipitation temperature is 80°C, and the reaction time is 0.5 h.
[0054] Example 10
[0055] The difference between Example 10 and Example 9 is that in step S3, the volume concentration of sulfur dioxide is 2 vol%.
[0056] Example 11
[0057] The difference between Example 11 and Example 1 is that in step S4, the endpoint pH of the solution system is controlled to be 8.5, the nickel precipitation temperature is 30° C., and the reaction time is 5 h.
[0058] Example 12
[0059] The difference between Example 12 and Example 1 is that in step S4, the endpoint pH of the solution system is controlled to be 7.5, the nickel precipitation temperature is 80° C., and the reaction time is 0.5 h.
[0060] Example 13
[0061] The difference between Example 13 and Example 1 is that in step S5, the crystallization temperature is 100° C. and the time is 0.5 h.
[0062] Example 14
[0063] The difference between Example 14 and Example 1 is that in step S5, the crystallization temperature is 70° C. and the time is 3 hours.
[0064] Comparative Example 1
[0065] The difference between Comparative Example 1 and Example 1 is that in step S2, potassium persulfate is added for oxidation.
[0066] Comparative Example 2
[0067] The difference between Comparative Example 2 and Example 1 is that in step S4, the endpoint pH of the solution system is controlled to be 6.0.
[0068] Comparative Example 3
[0069] The composition of the cobalt-containing rare earth wastewater (by mass concentration) is: 8 g / L cobalt, 0.8 g / L nickel, 5 g / L copper, 0.2 g / L rare earth elements, and a pH of 1. Lime milk was added to the cobalt-containing rare earth wastewater to adjust the pH to 7 and allow precipitation. The precipitate contains a mixture of copper, nickel, cobalt, and rare earth elements, making it impossible to calculate the recovery rate of each metal individually.
[0070] The recovery results of each metal element in Examples 1 to 14 and Comparative Examples 1 to 2 are shown in Table 1.
[0071] Table 1
[0072]
[0073]
[0074] As can be seen from the above, compared with the comparative example, each embodiment of the present invention first replaces and removes copper, then removes iron and aluminum and enriches rare earths, then oxidizes and precipitates cobalt, then chemically precipitates nickel, and finally recovers salt substances in the wastewater. By means of staged precipitation, the copper, rare earth, nickel, and cobalt metals therein are recovered step by step, and the products are sold and processed separately. The recovery cost is low, the recovery process is short, the recovery method is simple and easy to operate, the recovery of various metals is more thorough, the economic benefits are greatly improved, zero emissions are basically achieved, and environmental pollution is small.
[0075] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention are intended to be within the scope of protection of the present invention.
Claims
1. A method for recovering cobalt-containing rare earth waste liquid, characterized in that: The metal elements of the cobalt-containing rare earth waste liquid include copper, nickel, cobalt and rare earth elements, and the anions of the cobalt-containing rare earth waste liquid include chloride ions. The recovery method comprises the following steps: Step S1, adding a displacing agent to the cobalt-containing rare earth waste liquid to displace and remove copper, thereby obtaining sponge copper and a copper-removed liquid; Step S2, adding a first oxidant and lime milk to the copper-removed liquid in sequence, adjusting the pH to 4.0-5.0 to remove the displacing agent, and obtaining a displacing agent-rare earth mixed slag and a displacing agent-removed liquid; Step S3, sequentially adding a second oxidant and the lime milk to the liquid after the replacement agent is removed, adjusting the pH to 4.0-5.0 to precipitate cobalt, and obtaining a high-valent oxide of cobalt and a liquid after cobalt precipitation; Step S4, adding the lime milk to the cobalt precipitation solution to precipitate nickel, adjusting the pH to 7.5-8.5, and obtaining nickel hydroxide and nickel precipitation solution; Step S5, evaporating and crystallizing the nickel precipitation solution to obtain a crystalline salt, wherein the crystalline salt includes calcium chloride; Wherein, the replacement agent is iron powder and / or aluminum powder; and the oxidizing property of the first oxidant is lower than that of the second oxidant.
2. The recycling method according to claim 1, characterized in that: In the step S1, the dosage coefficient of the displacing agent is 1.0 to 5.
0.
3. The recycling method according to claim 2, characterized in that: The replacement temperature of step S1 is 30-80° C., and the replacement time is 5-120 min.
4. The recovery method according to any one of claims 1 to 3, characterized in that: In step S2, the first oxidant is one or more of hydrogen peroxide, oxygen and air.
5. The recovery method according to any one of claims 1 to 3, characterized in that: In the step S2, the dosage coefficient of the first oxidant is 1.0 to 2.
0.
6. The recycling method according to claim 5, characterized in that: The reaction temperature of step S2 is 30-80° C., and the reaction time is 0.5-5 h.
7. The recovery method according to any one of claims 1 to 3, characterized in that: In step S3, the second oxidant is one or more of persulfate, chlorate, sulfur dioxide and ozone.
8. The recycling method according to claim 7, characterized in that: The persulfate is one or more of potassium persulfate, sodium persulfate and calcium persulfate; the chlorate is one or more of potassium chlorate, sodium chlorate and calcium chlorate; the volume concentration of sulfur dioxide and / or ozone is 0.1-2 vol%.
9. The recovery method according to any one of claims 1 to 3, characterized in that: In the step S3, the dosage coefficient of the second oxidant is 1.0 to 2.
0.
10. The recycling method according to claim 9, characterized in that: The reaction temperature of step S3 is 30-80° C., and the reaction time is 0.5-5 h.
11. The recycling method according to claim 10, characterized in that: The reaction temperature of step S4 is 30-80° C., and the reaction time is 0.5-5 h.
12. The recovery method according to any one of claims 1 to 3, characterized in that: In the step S5, the temperature of the evaporation crystallization is 70-100° C., and the time is 0.5-3 hours.
13. The recovery method according to any one of claims 1 to 3, characterized in that: Measured by mass concentration, the cations in the cobalt-containing rare earth waste liquid include 8 to 15 g / L of cobalt ions, 0.5 to 3 g / L of nickel ions, 1 to 5 g / L of copper ions, and 0.01 to 1 g / L of rare earth element ions, and the rare earth element ions include one or more of Nd, Sm, Tb and Dy.
14. The recovery method according to any one of claims 1 to 3, characterized in that: The pH of the cobalt-containing rare earth waste liquid is 0.8-1.
2.
15. The recovery method according to any one of claims 1 to 3, characterized in that: The cobalt recovery rate in the cobalt-containing rare earth waste liquid is ≥99%, the nickel recovery rate is ≥98%, and the copper recovery rate is ≥92%.
Citation Information
Patent Citations
Processing method of trivalent cobalt nickel oxide waste material and waste cobalt nickel alloy
CN102952954A
Method for recovering rare earth, aluminum and silicon from rare earth-containing aluminum and silicon wastes