A polyurethane wiring harness encapsulation composite polyether and its preparation method and application

By combining materials such as polyether polyol and silicone surfactant to prepare polyurethane wire harness encapsulation, the problem of easy damage and poor performance of existing materials is solved, and a polyurethane foam material with high hardness and heat resistance is realized, which is suitable for automobiles. Electronic control system.

CN116082601BActive Publication Date: 2024-10-22HEBEI YADONG CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310041429.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-11
Publication Date
2024-10-22
Estimated Expiration
2043-01-11

AI Technical Summary

Technical Problem

Existing polyurethane wire harness encapsulation materials are easily damaged and occupy a large space in automotive electronic control systems, and the combined polyether preparation performance is poor and difficult to meet thermal stability and hardness requirements.

Method used

Polyether polyol I and polyether polyol II are combined with silicone surfactants, catalysts and chain extenders. The combined polyether is prepared by stirring, and mixed with Wannate 8019 and Wanante CDMDI100L of Wanhua Chemical. The foaming gun tip is injected into the mold to prepare polyurethane foam.

Benefits of technology

It improves the compatibility and hardness of the material, has excellent heat resistance and dimensional stability, meets the assembly requirements of automotive wiring harness encapsulation, and shows 58-65 ShoreA hardness, 260-380 kPa tensile strength and 40-52% elongation at break.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004050761990000081
    Figure BDA0004050761990000081
  • Figure BDA0004050761990000091
    Figure BDA0004050761990000091
Patent Text Reader

Abstract

The present invention relates to a polyurethane wiring harness encapsulation composite polyether and a preparation method and application thereof. The composite polyether raw materials include, by weight: 40-65 parts of polyether polyol I, 25-45 parts of polyether polyol II, 5-10 parts of chain extender, 0.3-1.5 parts of catalyst, 0.1-0.5 parts of silicon surfactant, 0.1-0.5 parts of water, and 2-5 parts of black slurry; the polyether polyol I, polyether polyol II, 1,4-butanediol, catalyst , silicone surfactant, the sum of water and black slurry is 100 parts; polyether polyol I has a functionality of 3, a hydroxyl value of 33-37 mgKOH / g, and a viscosity of 800-1200 mPa.s at 25°C; polyether polyol II has a functionality of 2, a hydroxyl value of 26-30 mgKOH / g, and a viscosity of 800-1000 mPa.s at 25°C. The polyurethane encapsulation material prepared by the combined polyether of the present invention has excellent heat resistance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyurethane wire harness encapsulated composite polyether and a preparation method and application thereof, belonging to the technical field of composite polyether. Background Art

[0002] With the continuous development of my country's automobile industry, electronic control systems are being applied in more and more scenarios, and the layout and appearance of electronic control systems have become a new direction of industry research. The wiring harness is mostly wrapped and organized in a corrugated tube. The wiring harness passes through the corrugated tube in a loose form. During the driving process of the car, the wiring harness and electrical components vibrate and rub in the corrugated tube, which is easy to be damaged. In addition, the corrugated tube is circular in design, occupies a large space, and is not easy to arrange.

[0003] Polyurethane foam is a material with excellent properties such as thermal insulation, water and moisture resistance, chemical resistance, good adhesion and long service life. For the current polyurethane automotive wiring harness encapsulation production line in China, high-pressure machines are mostly used to mix the raw materials and inject them into the mold. After a certain period of maturation, the product is taken out of the mold, and after passing the inspection of the inspection tool, it is stored and packaged for continuous production.

[0004] Since the wiring harness is arranged around or inside the engine, the polyurethane encapsulation material must have excellent thermal stability, and also have appropriate hardness and shrinkage to facilitate assembly. Combination polyether is one of the main raw materials for polyurethane, but the polyurethane wiring harness encapsulation prepared by current combination polyether has poor performance. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects in the prior art, provide a polyurethane wire harness encapsulation composite polyether and a preparation method thereof, and also provide a method for applying the polyurethane wire harness encapsulation composite polyether to polyurethane foam.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] Technical Theme 1

[0008] A polyurethane wire harness encapsulation composite polyether, the raw materials include, by weight: 40-65 parts of polyether polyol I, 25-45 parts of polyether polyol II, 5-10 parts of chain extender, 0.3-1.5 parts of catalyst, 0.1-0.5 parts of silicon surfactant, 0.1-0.5 parts of water, and 2-5 parts of black slurry;

[0009] The sum of the polyether polyol I, polyether polyol II, chain extender, catalyst, silicon surfactant, water and black slurry is 100 parts;

[0010] The polyether polyol I is a polyether polyol using glycerol as an initiator, having a functionality of 3, a hydroxyl value of 33-37 mgKOH / g, and a viscosity of 800-1200 mPa.s at 25°C;

[0011] The polyether polyol II is a polyether polyol using propylene glycol as an initiator, having a functionality of 2, a hydroxyl value of 26-30 mgKOH / g, and a viscosity of 800-1000 mPa.s at 25°C.

[0012] In some embodiments of the present invention, the catalyst is selected from one or a combination of any two or more of Huntsman's ZF10, Z130 and homemade A33; by mass percentage, the homemade A33 consists of 33% triethylenediamine and 67% propylene glycol.

[0013] In some embodiments of the present invention, the silicon-based surfactant is H695 from Dongjun Chemical.

[0014] In some embodiments of the present invention, the chain extender is selected from one or more of 1,4-butanediol, 1,3-butanediol and 2,3-dimethylbutanediol.

[0015] In some embodiments of the present invention, the chain extender is 1,4-butanediol and 2,3-dimethylbutanediol in a mass ratio of 1:0.5-1.1.

[0016] In some embodiments of the present invention, the black paste is 5U-506.

[0017] Technical Theme 2

[0018] A method for preparing a polyurethane wiring harness encapsulation composite polyether as provided in the first technical subject comprises the following steps:

[0019] Weigh polyether polyol I, polyether polyol II, chain extender, catalyst, silicon surfactant, water and black slurry, and then stir at 15-25° C., at a stirring rate of 800-1000 r / min, and for 40-60 min to obtain a composite polyether.

[0020] Technical Theme 3

[0021] An application of a polyurethane wire harness encapsulation combined polyether as provided in the technical subject one in the field of polyurethane foam, wherein the polyurethane foam raw material comprises component A and component B in a mass ratio of 100:30-45; the component A is the above-mentioned polyurethane wire harness encapsulation combined polyether, and the component B is Wannate 8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical.

[0022] In some embodiments of the present invention, the B component is Wannate 8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.4-0.8.

[0023] In some embodiments of the present invention, the method for preparing the polyurethane foam comprises the following steps:

[0024] The temperature is controlled at 25-28°C, and the gun head pressure is adjusted to 140-160 Bar. Component A and component B are mixed through the foaming gun head. The mixed material of component A and component B is injected into the mold through the gun head within 10 seconds, and taken out from the mold to obtain polyurethane foam.

[0025] In some embodiments of the present invention, the mold temperature is 50-55° C. and the demoulding time is 5-15 min.

[0026] The beneficial effects of adopting the above technical solution are:

[0027] The combined polyether provided by the present invention is a combination of polyether polyol I and polyether polyol II, and is matched with a silicone surfactant to enhance the compatibility of the entire system. It is also matched with a precisely matched catalyst and chain extender to prepare a polyurethane encapsulating material with suitable hardness, making the wiring harness easy to assemble, and has excellent heat resistance.

[0028] The polyurethane material obtained by the method provided by the present invention has been verified to have a polyurethane foam hardness of 58-65 (Shore A), heat aging: 2000 hours @ 120°C, tensile strength of 260-380 kPa, elongation at break of 40-52%, and tear strength of 120-145 kN / cm. The system has excellent heat resistance through the combination of polyether polyol structure, and it is also found that the system prepared by this combination has excellent dimensional stability. DETAILED DESCRIPTION

[0029] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is clearly and completely described below in conjunction with specific embodiments.

[0030] In the following examples, the polyether polyol I used is polyether polyol YD330N, provided by Hebei Yadong Chemical Group Co., Ltd.;

[0031] The polyether polyol II used was polyether polyol ED-28, provided by Shandong Bluestar Dongda Co., Ltd.;

[0032] The catalyst used is one of Z130, 2-[[2-[2-(dimethylamino)ethoxyethyl]methoxy]-ethanol (ZF10) and homemade A33 (33wt% triethylenediamine and 67wt% propylene glycol mixed) or a combination of any two or more thereof;

[0033] The silicon surfactant used was non-hydrolyzable silicon-carbon surfactant H695, provided by Zhongshan Dongjun Chemical Co., Ltd.; the black paste was 5U-506, provided by Jiali Chemical;

[0034] The B component used is Wannate 8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.4-0.8.

[0035] Example 1

[0036] Preparation of composite polyether:

[0037] By weight, 55.75 parts of polyether polyol I, 35 parts of polyether polyol II, 5 parts of 1,4-butanediol, 0.5 parts of catalyst, 0.5 parts of silicon surfactant, 0.25 parts of water, and 3 parts of black slurry were prepared as raw materials for standby use; then stirred at 25°C, with a stirring rate of 800 r / min and a stirring time of 60 min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.35 parts of A33;

[0038] Preparation of polyurethane wiring harness lagging:

[0039] The temperature was controlled at 25°C, and after the gun head pressure was adjusted to 160 Bar, component A and component B in a mass ratio of 100:30 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 50°C. After the product was matured, it was demolded. The demolding time was 15 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.4.

[0040] Example 2

[0041] Preparation of composite polyether:

[0042] According to weight, 55.8 parts of polyether polyol I, 35 parts of polyether polyol II, 5 parts of chain extender, 0.45 parts of catalyst, 0.5 parts of silicone surfactant, 0.25 parts of water, and 3 parts of black slurry were prepared as raw materials for standby use; then mixed and stirred at 15°C, with a stirring rate of 1000r / min and a stirring time of 40min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.30 parts of A33; the chain extender was 1,4-butanediol and 2,3-dimethylbutanediol in a mass ratio of 1:1;

[0043] Preparation of polyurethane wiring harness lagging:

[0044] The temperature was controlled at 28°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B in a mass ratio of 100:34 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 55°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.7.

[0045] Example 3

[0046] Preparation of composite polyether:

[0047] By weight, 55.8 parts of polyether polyol I, 35 parts of polyether polyol II, 5 parts of 1,4-butanediol, 0.45 parts of catalyst, 0.5 parts of silicon surfactant, 0.25 parts of water, and 3 parts of black slurry were prepared as raw materials for standby use; then mixed and stirred at 15°C, with a stirring rate of 1000 r / min and a stirring time of 40 min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.30 parts of A33;

[0048] Preparation of polyurethane wiring harness lagging:

[0049] The temperature was controlled at 28°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B in a mass ratio of 100:34 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 55°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.7.

[0050] Example 4

[0051] Preparation of composite polyether:

[0052] By weight, 55.8 parts of polyether polyol I, 35 parts of polyether polyol II, 5 parts of 2,3-dimethylbutanediol, 0.45 parts of catalyst, 0.5 parts of silicon surfactant, 0.25 parts of water, and 3 parts of black slurry were prepared as raw materials for standby use; then mixed and stirred at 15°C, with a stirring rate of 1000 r / min and a stirring time of 40 min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.30 parts of A33;

[0053] Preparation of polyurethane wiring harness lagging:

[0054] The temperature was controlled at 28°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B in a mass ratio of 100:34 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 55°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.7.

[0055] Example 5

[0056] Preparation of composite polyether:

[0057] By weight, 65 parts of polyether polyol I, 25 parts of polyether polyol II, 7.1 parts of 1,4-butanediol, 0.3 parts of catalyst, 0.1 parts of silicon surfactant, 0.5 parts of water, and 2 parts of black slurry were prepared as raw materials for standby use; then stirred at 15°C, with a stirring rate of 800r / min and a stirring time of 40min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.15 parts of A33;

[0058] Preparation of polyurethane wiring harness lagging:

[0059] The temperature was controlled at 25°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B in a mass ratio of 100:32 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 50°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.8.

[0060] Example 6

[0061] Preparation of composite polyether:

[0062] By weight, 40 parts of polyether polyol I, 45 parts of polyether polyol II, 7.9 parts of 1,3-butanediol, 1.5 parts of catalyst, 0.5 parts of silicon surfactant, 0.1 parts of water, and 5 parts of black slurry were prepared as raw materials for standby use; then stirred at 20°C, with a stirring rate of 800r / min and a stirring time of 40min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.7 parts of Z130 and 0.8 parts of A33;

[0063] Preparation of polyurethane wiring harness lagging:

[0064] The temperature was controlled at 25°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B in a mass ratio of 100:45 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 50°C. After the product was matured, it was demolded. The demolding time was 10 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.5.

[0065] Comparative Example 1

[0066] Preparation of composite polyether:

[0067] According to weight, 90.8 parts of polyether polyol I, 5 parts of chain extender, 0.45 parts of catalyst, 0.5 parts of silicon surfactant, 0.25 parts of water, and 3 parts of black slurry are prepared as raw materials for standby; then mixed and stirred at 15°C, with a stirring rate of 1000r / min and a stirring time of 40min to obtain a combined polyether, i.e., component A; the catalyst is composed of 0.15 parts of ZF10 and 0.30 parts of A33; the chain extender is 1,4-butanediol and 2,3-dimethylbutanediol in a mass ratio of 1:1;

[0068] Preparation of polyurethane wiring harness lagging:

[0069] The temperature was controlled at 28°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B in a mass ratio of 100:34 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 55°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.7.

[0070] Comparative Example 2

[0071] Preparation of composite polyether:

[0072] According to weight, 90.8 parts of polyether polyol II, 5 parts of chain extender, 0.45 parts of catalyst, 0.5 parts of silicon surfactant, 0.25 parts of water, and 3 parts of black slurry were prepared as raw materials for standby use; then mixed and stirred at 15°C, with a stirring rate of 1000r / min and a stirring time of 40min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.30 parts of A33; the chain extender was 1,4-butanediol and 2,3-dimethylbutanediol in a mass ratio of 1:1;

[0073] Preparation of polyurethane wiring harness lagging:

[0074] The temperature was controlled at 28°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B in a mass ratio of 100:34 were mixed through the foaming gun head, and the mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 55°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; wherein component B was Wannate8019 of Wanhua Chemical and Wanante CDMDI100L of Wanhua Chemical in a mass ratio of 1:0.7.

[0075] Comparative Example 3

[0076] Preparation of composite polyether:

[0077] According to weight, 55.8 parts of polyether polyol I, 35 parts of polyether polyol II, 5 parts of chain extender, 0.45 parts of catalyst, 0.5 parts of silicone surfactant, 0.25 parts of water, and 3 parts of black slurry were prepared as raw materials for standby use; then mixed and stirred at 15°C, with a stirring rate of 1000r / min and a stirring time of 40min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.30 parts of A33; the chain extender was 1,4-butanediol and 2,3-dimethylbutanediol in a mass ratio of 1:1;

[0078] Preparation of polyurethane wiring harness lagging:

[0079] The temperature was controlled at 28°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B with a mass ratio of 100:34 were mixed through the foaming gun head. The mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 55°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; component B was Wannate 8019 from Wanhua Chemical.

[0080] Comparative Example 4

[0081] Preparation of composite polyether:

[0082] According to weight, 55.8 parts of polyether polyol I, 35 parts of polyether polyol II, 5 parts of chain extender, 0.45 parts of catalyst, 0.5 parts of silicone surfactant, 0.25 parts of water, and 3 parts of black slurry were prepared as raw materials for standby use; then mixed and stirred at 15°C, with a stirring rate of 1000r / min and a stirring time of 40min to obtain a combined polyether, i.e., component A; the catalyst was composed of 0.15 parts of ZF10 and 0.30 parts of A33; the chain extender was 1,4-butanediol and 2,3-dimethylbutanediol in a mass ratio of 1:1;

[0083] Preparation of polyurethane wiring harness lagging:

[0084] The temperature was controlled at 28°C, and after the gun head pressure was adjusted to 140 Bar, component A and component B with a mass ratio of 100:34 were mixed through the foaming gun head. The mixed material of component A and component B was injected into the mold through the gun head within 10 seconds. The mold temperature was 55°C. After the product was matured, it was demolded. The demolding time was 5 minutes to obtain polyurethane foam; component B was Wanante CDMDI100L of Wanhua Chemical.

[0085] Performance test

[0086] The polyurethane wire harness rubber obtained in Examples 1-6 and Comparative Examples 1-4 was subjected to a performance test, wherein the linear shrinkage was tested according to 3.2 post-shrinkage in GB / T 39818-2021, the heat treatment temperature was 80±2°C, the heat treatment time was 168h±2h, and the results were as shown in Table 1:

[0087] Table 1

[0088]

[0089]

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An application of a polyurethane wire harness encapsulation composite polyether in the field of polyurethane foam, characterized in that: The polyurethane foam raw material comprises component A and component B in a mass ratio of 100:30-45; The B component is Wannate 8019 of Wanhua Chemical and WananteCDMDI100L of Wanhua Chemical in a mass ratio of 1:0.4-0.8; The component A is a polyurethane wire harness adhesive composite polyether, and the raw materials of the polyurethane wire harness adhesive composite polyether include, by weight: 40-65 parts of polyether polyol I, 25-45 parts of polyether polyol II, 5-10 parts of chain extender, 0.3-1.5 parts of catalyst, 0.1-0.5 parts of silicon surfactant, 0.1-0.5 parts of water, and 2-5 parts of black slurry; The sum of the polyether polyol I, polyether polyol II, chain extender, catalyst, silicon surfactant, water and black slurry is 100 parts; The polyether polyol I is a polyether polyol using glycerol as an initiator, having a functionality of 3, a hydroxyl value of 33-37 mgKOH / g, and a viscosity of 800-1200 mPa.s at 25°C; The polyether polyol II is a polyether polyol with propylene glycol as the initiator, a functionality of 2, a hydroxyl value of 26-30 mgKOH / g, and a viscosity of 800-1000 mPa.s at 25°C; The chain extender is 1,4-butanediol and 2,3-dimethylbutanediol in a mass ratio of 1:0.5-1.

1.

2. The application of the polyurethane wire harness encapsulation composite polyether in the field of polyurethane foam according to claim 1, characterized in that: The catalyst is selected from one of Huntsman's ZF10, Z130 and homemade A33, or a combination of any two or more thereof; in terms of mass percentage, the homemade A33 is composed of 33% triethylenediamine and 67% propylene glycol.

3. The application of the polyurethane wire harness encapsulation composite polyether in the field of polyurethane foam according to claim 1, characterized in that: The silicon surfactant is H695 produced by Dongjun Chemical; the black paste is 5U-506.

4. The application of the polyurethane wire harness encapsulation composite polyether in the field of polyurethane foam according to claim 1, characterized in that: The preparation method of the polyurethane wiring harness encapsulated composite polyether comprises the following steps: Weigh polyether polyol I, polyether polyol II, chain extender, catalyst, silicon surfactant, water and black slurry according to the mass fractions of claim 1, and then mix and stir at 15-25° C., at a stirring rate of 800-1000 r / min, and for 40-60 min to obtain a composite polyether.

5. The use of a polyurethane wire harness encapsulation composite polyether in the field of polyurethane foam according to claim 4, characterized in that: The preparation method of the polyurethane foam comprises the following steps: The temperature is controlled at 25-28°C, and the gun head pressure is adjusted to 140-160Bar. Component A and component B are mixed through the foaming gun head. The mixed material of component A and component B is injected into the mold through the gun head within 10 seconds, and demolded to obtain polyurethane foam.

6. The use of a polyurethane wire harness encapsulation composite polyether in the field of polyurethane foam according to claim 5, characterized in that: The mold temperature is 50-55° C., and the demoulding time is 5-15 min.