Preparation method of biodegradable copolyester with both flame retardant and plasticizing functions
Through the oxidation reaction of itaconic acid and the ring-opening addition of CO2 to form a cross-linked network structure, combined with the copolymerization of phosphorus-containing hydroxy acids, the problem of insufficient mechanical properties and heat resistance of biodegradable aliphatic polyester materials has been solved, and high compatibility and mechanical properties have been achieved. Improved performance and enhanced biodegradability.
Patent Information
- Application Number
- CN202310053900.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-03
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-02-03
AI Technical Summary
Biodegradable aliphatic polyester materials have deficiencies in mechanical properties, processability and heat resistance, and differences in plasticizer molecular structures lead to phase separation and poor compatibility.
Itaconic acid is used to synthesize epoxy compound monomers through oxidation reaction, and through CO2 ring-opening addition reaction and esterification-condensation polymerization reaction of alcohol and acid, a cross-linked biodegradable copolyester material is formed, combined with phosphorus-containing hydroxy acid Copolymerize to form a cross-linked network structure connected by chemical bonds.
It significantly improves the compatibility, mechanical properties and heat resistance of copolyester materials, enhances biodegradability through cross-linked network structure, increases toughness and flame retardant properties, and expands the scope of applications.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material synthesis, and in particular relates to a method for preparing a biodegradable copolyester having both flame retardant and plasticizing functions. Background Art
[0002] At present, biodegradable aliphatic polyester materials (such as polylactic acid, polybutylene succinate, etc.) have been widely used in product packaging, agricultural films, tableware production and medical materials. However, aliphatic polyesters often have poor mechanical properties, and injection molding processability and heat resistance are difficult to meet the requirements of various uses. To this end, toughening agents such as phosphate esters, petroleum esters, and polyesters are usually added for blending and modification to solve this problem. However, due to the difference in the molecular structure of the plasticizer, phase separation is easily caused, and compatibility is deteriorated. The Chinese patent (patent number: ZL201910510635.9) proposes a PBS composite material containing a PBSM toughening agent and a preparation method thereof. First, succinic acid, butanediol, and isoprene glycol are used as raw materials, and a PBSM polyester plasticizer with a molecular chain structure similar to that of PBS is prepared by esterification-polycondensation reaction; then PBS and PBSM are melt-blended to obtain the composite material. This technology improves the compatibility of polyester to a certain extent, but no chemical bonds are generated between the molecular chains of the two resins, and the improvement of the mechanical properties and heat resistance of the polyester is not obvious. Summary of the invention
[0003] In view of the problems existing in the background technology, the present invention provides a method for preparing a biodegradable copolyester having both flame retardant and plasticizing functions.
[0004] The technical solution adopted by the present invention includes the following characteristic steps:
[0005] 1. Add itaconic acid to a polyester reactor, while stirring, introduce nitrogen to exhaust the air in the reactor, then add a catalyst and slowly introduce ozone gas (O3), wherein: the mass ratio of the catalyst to itaconic acid is 0.002-0.008:1, and the molar ratio of ozone to itaconic acid is 1-2:1; then quickly heat the system to 40°C-60°C for oxidation reaction, and when the ozone gas is completely introduced, cool to room temperature to stop the reaction, and obtain an itaconic acid epoxidation monomer;
[0006] The catalyst described in step 1 is a titanium-based catalyst, and the preparation method is the same as one of the Chinese invention patents (patent number: ZL201910994074.4) or Chinese invention patents (patent number: ZL201910947191.5);
[0007] 2. Continuously charge CO2 into the catalyst-containing product obtained in step 1 until the system pressure is 4.5-5.5 MPa and keep the system pressure unchanged, then add hydroxyphosphonic acid and butanediol, wherein the molar ratio of hydroxyphosphonic acid to itaconic acid is 0.5-2.0:1, and the molar ratio of butanediol to itaconic acid is 3.0-5.0:1; heat the system to 140°C-160°C under rapid stirring to carry out ring-opening addition reaction and esterification reaction, and take the time when the first drop of esterification water is distilled out as the zero point of the esterification reaction timing, react at this temperature for 1-2 hours, and when the distilled water is obviously very little, the reaction is completed;
[0008] In step 2, the hydroxyphosphonic acid is one of hydroxyethylidene diphosphonic acid or 2-hydroxyphosphonoacetic acid; its molecular formula is as follows:
[0009] (Hydroxyethylidene diphosphonic acid, HEDP)
[0010] (2-Hydroxyphosphonoacetic acid, HPAA)
[0011] 3. Evacuate the system and maintain the vacuum state at a vacuum degree of 50-100 Pa; then heat the system to 180°C-200°C for polycondensation reaction. When the intrinsic viscosity of the reaction product (measured by Ubbelohde viscometer at 25°C) is 1.0-1.5 dL·g -1 The material is discharged when the reaction product is cooled by cold water and then cut into polyester slices, thereby obtaining a biodegradable copolyester with both flame retardant and plasticizing functions.
[0012] Beneficial effects of the present invention:
[0013] (1) The present invention first uses biodegradable itaconic acid as a raw material, synthesizes epoxy compound monomers through gas O3 oxidation reaction, and then prepares a cross-linked biodegradable copolyester material with both flame retardant and plasticizing functions through CO2 ring-opening addition reaction and alcohol and acid esterification-polycondensation reaction. The material has the excellent properties of polycarbonate and phosphorus-containing aliphatic polyester, wherein the polycarbonate molecular chain and the phosphorus-containing aliphatic polyester molecular chain are bonded to form a cross-linked network structure in the form of chemical bonds. On the one hand, the compatibility, mechanical properties and heat resistance of the copolyester material are greatly improved, and its comprehensive performance is improved; on the other hand, the cross-linked network structure can form a large number of molecular internal cavity structures, which is conducive to the entry of microorganisms, acid and alkaline ions in nature into the cavity, further improving the biodegradability of the copolyester material.
[0014] (2) The present invention selects a phosphorus-containing hydroxy acid to copolymerize with an aliphatic dibasic acid and a diol, which has the following advantages: ① Usually, the cross-linking reaction increases the molecular weight of the polyester, resulting in poor toughness. The phosphorus-containing hydroxy acid is an effective plasticizer that can improve the toughness of the cross-linked copolyester; ② The addition of the phosphorus-containing hydroxy acid to the copolymerization makes the copolyester contain phosphorus-carbon (PC) bonds on the molecular chain, so that the prepared copolyester has flame retardant properties, thereby expanding its application range.
[0015] (3) The itaconic acid used in the present invention as a raw material can be produced by various means such as biomass fermentation and petroleum refining, and has the advantages of good biodegradability and a wide range of sources. DETAILED DESCRIPTION
[0016] Example 1
[0017] 1. Add 1.0 kg of itaconic acid into a polyester reactor, while stirring, introduce nitrogen to expel the air in the reactor, then add 0.002 kg of a titanium catalyst, and slowly introduce 172.1 liters of ozone gas, then quickly heat the system to 40°C for oxidation reaction, and after the ozone gas is introduced, cool to room temperature to stop the reaction, and obtain an itaconic acid epoxidation monomer;
[0018] 2. Continuously charge CO2 into the product containing the titanium-based catalyst obtained in step 1 until the system pressure reaches 5.5 MPa and keep the system pressure unchanged, then add 0.79 kg of hydroxyethylidene diphosphonic acid and 2.08 kg of butanediol; heat the system to 140°C under rapid stirring conditions to carry out ring-opening addition reaction and esterification reaction, and use the time when the first drop of esterification water is distilled out as the zero point of the esterification reaction timing, react at this temperature for 2 hours, and when the distilled water is obviously very little, the reaction is completed;
[0019] 3. The system was evacuated and maintained at a vacuum degree of 50 Pa. The system was heated to 200°C for polycondensation. When the intrinsic viscosity of the reaction product (measured by an Ubbelohde viscometer at 25°C) was 1.0 dL·g -1 The material is discharged when the reaction product is cooled by cold water and then cut into polyester slices, thereby obtaining a biodegradable copolyester with both flame retardant and plasticizing functions.
[0020] Example 2
[0021] 1. Add 1.0 kg of itaconic acid into a polyester reactor, while stirring, introduce nitrogen to expel the air in the reactor, then add 0.008 kg of a titanium catalyst, and slowly introduce 344.4 liters of ozone gas, then quickly heat the system to 60°C for oxidation reaction, and after the ozone gas is introduced, cool to room temperature to stop the reaction, and obtain an itaconic acid epoxidation monomer;
[0022] 2. Continuously charge CO2 into the product containing the titanium-based catalyst obtained in step 1 until the system pressure reaches 4.5 MPa and keep the system pressure constant, then add 2.40 kg of 2-hydroxyphosphonoacetic acid and 3.46 kg of butanediol; heat the system to 160° C. under rapid stirring conditions to carry out ring-opening addition reaction and esterification reaction, and use the time when the first drop of esterification water is distilled out as the zero point of the esterification reaction timing, react at this temperature for 1 hour, and when the distilled water is significantly less, the reaction is completed;
[0023] 3. The system was evacuated and maintained at a vacuum degree of 100 Pa. The system was heated to 180°C for polycondensation. When the intrinsic viscosity of the reaction product (measured by an Ubbelohde viscometer at 25°C) was 1.5 dL·g -1 The material is discharged when the reaction product is cooled by cold water and then cut into polyester slices, thereby obtaining a biodegradable copolyester with both flame retardant and plasticizing functions.
[0024] Example 3
[0025] 1. Add 1.0 kg of itaconic acid into a polyester reactor, while stirring, introduce nitrogen to expel the air in the reactor, then add 0.005 kg of a titanium catalyst, and slowly introduce 258.3 liters of ozone gas, then quickly heat the system to 50°C for oxidation reaction, and after the ozone gas is introduced, cool to room temperature to stop the reaction, and obtain an itaconic acid epoxidation monomer;
[0026] 2. Continuously charge CO2 into the product containing the titanium-based catalyst obtained in step 1 until the system pressure reaches 5.0 MPa and keep the system pressure unchanged, then add 1.20 kg of 2-hydroxyphosphonoacetic acid and 2.77 kg of butanediol; heat the system to 120° C. under rapid stirring to carry out ring-opening addition reaction and esterification reaction, and take the time when the first drop of esterification water is distilled out as the zero point of the esterification reaction timing, react at this temperature for 1.5 hours, and when the distilled water is obviously very little, the reaction is completed;
[0027] 3. The system was evacuated and maintained at a vacuum degree of 75 Pa. The system was heated to 190°C for polycondensation. When the intrinsic viscosity of the reaction product (measured by an Ubbelohde viscometer at 25°C) was 1.25 dL·g -1 The material is discharged when the reaction product is cooled by cold water and then cut into polyester slices, thereby obtaining a biodegradable copolyester with both flame retardant and plasticizing functions.
[0028] Example 4
[0029] 1. Add 1.0 kg of itaconic acid into a polyester reactor, while stirring, introduce nitrogen to expel the air in the reactor, then add 0.006 kg of a titanium catalyst, and slowly introduce 310.0 liters of ozone gas, then quickly heat the system to 55°C for oxidation reaction, and after the ozone gas is introduced, cool to room temperature to stop the reaction, and obtain an itaconic acid epoxidation monomer;
[0030] 2. Continuously charge CO2 into the product containing the titanium-based catalyst obtained in step 1 until the system pressure reaches 5.0 MPa and keep the system pressure unchanged, then add 2.38 kg of hydroxyethylidene diphosphonic acid and 3.12 kg of butanediol; heat the system to 130° C. under rapid stirring conditions to carry out ring-opening addition reaction and esterification reaction, and use the time when the first drop of esterification water is distilled out as the zero point of the esterification reaction timing, react at this temperature for 1.5 hours, and when the distilled water is obviously very little, the reaction is completed;
[0031] 3. The system was evacuated and maintained at a vacuum degree of 80 Pa. The system was heated to 185°C for polycondensation. When the intrinsic viscosity of the reaction product (measured by an Ubbelohde viscometer at 25°C) was 1.3 dL·g -1 The material is discharged when the reaction product is cooled by cold water and then cut into polyester slices, thereby obtaining a biodegradable copolyester with both flame retardant and plasticizing functions.
[0032] Comparative Example 1
[0033] In Comparative Example 1, the process of introducing ozone and CO2 gas in Example 4 was removed, and other process conditions remained unchanged. The specific operation steps were as follows:
[0034] 1. Add 1.0 kg of itaconic acid into a polyester reactor, while stirring, introduce nitrogen to expel the air in the reactor, then add 0.006 kg of titanium catalyst, 2.38 kg of hydroxyethylidene diphosphonic acid and 3.12 kg of butanediol; heat the system to 130°C under rapid stirring conditions to carry out esterification reaction, and take the time when the first drop of esterification water is distilled out as the zero point of the esterification reaction timing, react at this temperature for 1.5 hours, and when the distilled water is obviously very little, the reaction is completed;
[0035] 3. The system was evacuated and maintained at a vacuum degree of 80 Pa. The system was heated to 185°C for polycondensation. When the intrinsic viscosity of the reaction product (measured by an Ubbelohde viscometer at 25°C) was 1.3 dL·g -1 The material is discharged when the reaction product is cooled by cold water and then cut into polyester slices, thereby obtaining a biodegradable copolyester with both flame retardant and plasticizing functions.
[0036] Comparative Example 2
[0037] In Comparative Example 2, the hydroxyphosphonic acid step added in Example 4 was removed, and other process conditions remained unchanged. The specific operation steps were as follows:
[0038] 1. Add 1.0 kg of itaconic acid into a polyester reactor, while stirring, introduce nitrogen to expel the air in the reactor, then add 0.006 kg of a titanium catalyst, and slowly introduce 310.0 liters of ozone gas, then quickly heat the system to 55°C for oxidation reaction, and after the ozone gas is introduced, cool to room temperature to stop the reaction, and obtain an itaconic acid epoxidation monomer;
[0039] 2. Continuously charge CO2 into the product containing the titanium-based catalyst obtained in step 1 until the system pressure reaches 5.0 MPa and keep the system pressure unchanged, then add 3.12 kg of butanediol; heat the system to 130° C. under rapid stirring conditions to carry out ring-opening addition reaction and esterification reaction, with the time when the first drop of esterification water is distilled out as the zero point of the esterification reaction timing, react at this temperature for 1.5 hours, and when the distilled water is significantly less, the reaction is completed;
[0040] 3. The system was evacuated and maintained at a vacuum degree of 80 Pa. The system was heated to 185°C for polycondensation. When the intrinsic viscosity of the reaction product (measured by an Ubbelohde viscometer at 25°C) was 1.3 dL·g -1 The material is discharged when the reaction product is cooled by cold water and then cut into polyester chips, thereby obtaining a biodegradable copolyester.
[0041] Performance Evaluation
[0042] The flame retardancy, tensile strength and biodegradability of the samples prepared in the embodiments and comparative examples are comprehensively evaluated. The results are shown in Table 1.
[0043] Flame retardant performance test: Oxygen index (LOI) is tested according to ASTM D2863 standard; comprehensive vertical combustion (UL-94) is tested according to ASTM D3801 standard.
[0044] Tensile strength test: The polyesters prepared in the examples and comparative examples were tested for tensile strength according to the national standard GB / T1040.2-2006 using an electronic universal testing machine (CMT5104, Shenzhen Xinsansi Metrology Technology Co., Ltd.).
[0045] Test of polyester biodegradability: The polyester chips prepared in the examples and comparative examples were made into 30 mm×30 mm×2 mm plate samples and buried in slightly acidic (pH=4) compost. After 20 weeks, the weight loss rate was measured.
[0046] Table 1
[0047] name Oxygen Index (LOI) Vertical burning rating (UL-94) Tensile strength / MPa Weight loss rate / % Example 1 30 V-1 26.1 5.3 Example 2 33 V-1 25.3 5.6 Example 3 31 V-1 25.8 5.5 Example 4 34 V-0 26.4 5.8 Comparative Example 1 29 V-1 11.2 3.1 Comparative Example 2 24 none 24.7 2.7
Claims
1. A method for preparing a biodegradable copolyester having both flame retardant and plasticizing functions, characterized in that: (1) adding itaconic acid to a reactor, stirring while introducing nitrogen to expel air in the reactor, then adding a catalyst and slowly introducing ozone gas, and heating to 40°C to 60°C for oxidation reaction. After the ozone gas is introduced, cooling to room temperature stops the reaction, and obtaining a catalyst-containing itaconic acid epoxidation monomer; the catalyst is a titanium-based catalyst; the mass ratio of the catalyst to itaconic acid is 0.002 to 0.008:1; the molar ratio of ozone to itaconic acid is 1 to 2:1; (2) continuously charging CO2 into the catalyst-containing itaconic acid epoxidation monomer obtained in step 1 until the system pressure is 4.5-5.5 MPa and maintaining the system pressure constant, then adding hydroxyphosphonic acid and butanediol, and heating the system to 140° C.-160° C. under stirring to carry out ring-opening addition reaction and esterification reaction; the hydroxyphosphonic acid is hydroxyethylidene diphosphonic acid or 2-hydroxyphosphonoacetic acid; (3) After the reaction in step (2), the reaction system is evacuated and maintained in a vacuum state, and then the system is heated to 180°C to 200°C for polycondensation reaction. When the reaction product reaches a certain characteristic viscosity, the material is discharged. After the reaction product is cooled, it is sliced to obtain a biodegradable copolyester having both flame retardant and plasticizing functions.
2. The method for preparing the biodegradable copolyester having both flame retardant and plasticizing functions according to claim 1, characterized in that: The molar ratio of the hydroxyphosphonic acid to itaconic acid is 0.5-2.0:1; the molar ratio of butanediol to itaconic acid is 3.0-5.0:
1.
3. The method for preparing the biodegradable copolyester having both flame retardant and plasticizing functions according to claim 1, characterized in that: The reaction time of step (2) is 1 to 2 hours, with the first drop of esterification water distilled out as the zero point of the esterification reaction.
4. The method for preparing the biodegradable copolyester having both flame retardant and plasticizing functions according to claim 1, characterized in that: The step (3) is to evacuate to a vacuum degree of 50-100 Pa; the intrinsic viscosity of the material is in the range of 1.0-1.5 dL·g -1 .
Citation Information
Patent Citations
PBS composite material containing PBSM toughening agent and preparation method thereof
CN110240788A
Preparation method and application of green titanium polyester catalyst
CN110606946A
Preparation method and application of rod-shaped amorphous / anatase type TiO2 composite catalyst
CN110724254A
Phosphorus-containing PTT fire-resistant copolyesters / nano composite material and preparation method thereof
CN101709137A
Biologic polycarbonate and preparation method thereof
CN102585192A